Glazed glaze, multi-layer antique inkjet brick and preparation method thereof

By adjusting the glaze composition and multi-layer design, the problems of poor color and insufficient three-dimensionality of the glaze of antique bricks are solved, and the stability and layering are improved, giving antique bricks better gloss and imitation effects.

CN118930047AActive Publication Date: 2024-11-12ZHUHAI DOUMEN DISTRICT XURI CERAMICS CO LTD

Patent Information

Application Number
CN202410849424.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-12
Estimated Expiration
2044-06-27

AI Technical Summary

Technical Problem

The glaze of existing antique bricks has poor color performance, resulting in unstable combination of ink and glaze, causing the problem of dispersing and dispersing, and lacking three-dimensionality and layering.

Method used

A glossy glaze is used to adjust the content of calcite, zinc oxide and quartz to ensure the appropriate high temperature viscosity of the glaze. Combined with the design of the bottom glaze layer, the dot glaze layer and the inkjet layer, it forms multi-layer antique inkjet bricks. Use point-swinging technology and inkjet technology to create concave and convex textures and color changes to enhance layering and three-dimensionality.

Benefits of technology

The stability of the glaze and the normality of ink color are achieved, the gloss and wear resistance of the bricks are enhanced, and the antique bricks are given a strong sense of layering and three-dimensionality, which enhances the authenticity of its imitation stone effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930047A_ABST
    Figure CN118930047A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of ceramic tiles, in particular to glazed glaze, a multi-layer antique inkjet brick and a preparation method of the multi-layer antique inkjet brick. The glazed glaze is prepared from the following raw materials in percentage by mass: 40%-46% of high-temperature potassium feldspar, 2%-5% of calcite, 3%-8% of black mud, 13%-18% of quartz, 20%-26% of barium carbonate, 3%-8% of raw kaolin, 3%-8% of zinc oxide, 0.2%-0.3% of sodium tripolyphosphate and 1.3%-1.7% of carboxymethyl cellulose. The glazed glaze is appropriate in high-temperature viscosity, good in ink color development, high in hardness after being sintered and good in wear resistance. The invention also provides a multi-layer antique ink-jet brick which is prepared by adopting a glaze throwing process and has strong hierarchy and good stereoscopic impression.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic tiles, and in particular to a glossy glazed, multi-layered antique inkjet tile and a preparation method thereof. Background Art

[0002] With the development of large-scale and rapid inkjet technology, people have a growing demand for artistic decorations. Antique tiles are actually glazed porcelain tiles, often used for building walls and floors. Because of their patterns and textures, they have a similar effect to stone veneers after a long period of time, full of the vicissitudes of time and the heaviness of history. Therefore, antique tiles often create a nostalgic atmosphere through the combination of styles, colors and patterns. Antique tiles evolved from colored glazed tiles. Compared with ordinary glazed tiles, the difference is mainly reflected in the color of the glaze.

[0003] At present, the patterns and colors of traditional antique tiles are already very rich, but they generally lack layering and three-dimensionality. The main reason is that the glossiness of the glaze of antique tiles is basically the same, and the formation of three-dimensionality and layering can only rely on the color and pattern design of the inkjet process, which results in the antique tiles imitating the traces of stone use. The effect is not good.

[0004] In addition, existing glazes such as glossy glaze have poor color development properties, resulting in instability after the ink and glaze are combined, causing problems such as breaking up and blurring, and the color of the ink after firing does not meet expectations.

[0005] It can be seen that the existing technology still needs to be improved and enhanced. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a glossy glaze, multi-layered antique inkjet brick and a preparation method thereof, aiming to solve the technical problems in the prior art of poor color development of glaze and weak three-dimensional and layered effects of inkjet antique bricks.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] The first aspect of the present invention provides a bright glaze, wherein the raw materials for preparing the bright glaze include, by mass percentage: 40% to 46% of high-temperature potassium feldspar, 2% to 5% of calcite, 3% to 8% of black mud, 13% to 18% of quartz, 20% to 26% of barium carbonate, 3% to 8% of raw kaolin, and 3% to 8% of zinc oxide.

[0009] The second aspect of the present invention provides a multi-layer antique inkjet brick, which includes a body layer, a base glaze layer, an intermediate glaze layer, a glaze layer and an inkjet layer arranged in sequence; the intermediate glaze layer is made of the above-mentioned glossy glaze.

[0010] The multi-layered antique inkjet brick, wherein, by mass percentage, the raw materials for preparing the bottom glaze layer include: 8% to 14% high-temperature slurry, 4% to 8% zinc oxide, 13% to 15% zirconium silicate, 10% to 15% washed mud, 5% to 8% black mud powder, 35% to 40% red potassium sand, 8% to 10% burnt earth, 1% to 4% potassium feldspar, and 2% to 8% sodium soil.

[0011] The multi-layered antique inkjet brick, wherein, by mass percentage, the raw materials for preparing the high-temperature slurry include: 22% to 28% of waste materials, 15% to 20% of potassium feldspar, 13% to 18% of sodium feldspar, 8% to 12% of black mud powder, 8% to 12% of quartz, and 18% to 24% of kaolin.

[0012] The multi-layered antique inkjet brick, wherein, by mass percentage, the raw materials for preparing the glaze layer include: 23% to 30% of albite, 12% to 18% of high-temperature potassium feldspar, 10% to 15% of calcite, 5% to 8% of burned talc, 5% to 10% of black mud, 10% to 12% of burned kaolin, 2% to 5% of calcined zinc oxide, and 13% to 18% of barium carbonate.

[0013] The third aspect of the present invention provides a method for preparing an antique inkjet brick, which is used to prepare the multi-layer antique inkjet brick described above, comprising the following steps:

[0014] S001. Applying white glaze on the body layer to form a bottom glaze layer;

[0015] S002. Applying a glossy glaze to form an intermediate glaze layer;

[0016] S003. Apply matte glaze and grind glaze by throwing point process to form a throwing point glaze layer;

[0017] S004. Inkjet to form an inkjet layer;

[0018] S005. Firing, the sintering temperature is 1225°C to 1230°C, and the firing cycle is 50 to 55 minutes.

[0019] The method for preparing the antique inkjet brick, wherein the specific gravity of the white glaze slurry is 1.33-1.35 g / cm 3 ; The flow rate of the white glaze is 19 to 21 seconds; the flow rate of the glossy glaze is 19 to 21 seconds; the flow rate of the matte glaze is 19 to 21 seconds.

[0020] The method for preparing the antique inkjet brick, wherein the glaze slurry specific gravity of the glossy glaze is 1.33-1.35 g / cm 3 .

[0021] The method for preparing the antique inkjet brick, wherein the glaze slurry specific gravity of the matte glaze is 1.33-1.35 g / cm 3 .

[0022] The method for preparing antique inkjet bricks, wherein, in the throwing-off process, the frequency of the throwing-off cabinet is 3-7 Hz, and the speed of the conveyor belt is 14-16 cm / s.

[0023] Beneficial effects: The first aspect of the present invention provides a glossy glaze, wherein the glossy glaze adjusts the content of calcite and zinc oxide to make the high-temperature viscosity of the glaze appropriate, thereby ensuring that the ink has normal color and good gloss. In addition, by adjusting the amount of quartz, it is ensured that the glaze layer has sufficient hardness and wear resistance.

[0024] The second aspect of the present invention provides a multi-layered antique inkjet brick, which includes a body layer, a base glaze layer, an intermediate glaze layer, a throwing glaze layer and an inkjet layer arranged in sequence, wherein the intermediate glaze layer is made of the glossy glaze described above, and through the combination of the intermediate glaze layer, the throwing glaze layer and the inkjet layer, the intermediate glaze layer can have both concave and convex textures and color depth changes, which is rich in layering and three-dimensional sense.

[0025] The third aspect of the present invention provides a method for preparing antique inkjet bricks, which is used to prepare the above-mentioned multi-layer antique inkjet bricks. The preparation method first applies a base glaze and a glossy glaze on the body layer in sequence, then applies a matte glaze by a throwing point process, and finally inkjet fires. By matching the glossy glaze and the matte glaze, an antique inkjet brick with a strong sense of layering is formed. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a physical picture of Example 1.

[0027] Figure 2 This is a physical picture of Comparative Example 1.

[0028] Figure 3 This is a physical picture of Comparative Example 2. DETAILED DESCRIPTION

[0029] The present invention provides a glossy glaze, multi-layered antique inkjet brick and a preparation method thereof. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] The first aspect of the present invention provides a bright glaze, wherein the raw materials for preparing the bright glaze include, by mass percentage: 40% to 46% of high-temperature potassium feldspar, 2% to 5% of calcite, 3% to 8% of black mud, 13% to 18% of quartz, 20% to 26% of barium carbonate, 3% to 8% of raw kaolin, and 3% to 8% of zinc oxide.

[0031] Compared with the existing glossy glaze, the glossy glaze provided by the present invention can well maintain the stability of inkjet ink in the glaze without the phenomenon of being scattered and blurred; moreover, this formula has excellent color development ability for the ink, the surface of the glaze is smooth, the hand feel is delicate, and the anti-fouling ability is strong.

[0032] Specifically, the calcite and zinc oxide content in the glossy glaze cannot be too high. Too high a content will make its high-temperature viscosity too low. When preparing multi-layer antique inkjet tiles, it will dissolve the upper glaze layer, making the product lack layering and three-dimensionality, and will corrode the ink, making the ink color worse, and also affecting the glossiness of the product surface. The quartz content cannot be too low. Quartz is the skeleton of ceramics. Too little quartz will make the hardness and wear resistance of the product unqualified.

[0033] The second aspect of the present invention provides a multi-layer antique inkjet brick, which includes a body layer, a bottom glaze layer, an intermediate glaze layer, a glaze layer and an inkjet layer arranged in sequence; the intermediate glaze layer is made of the above-mentioned glossy glaze. The use of the glossy glaze ensures the uneven effect of the glaze layer and can ensure the color of the ink, so that the multi-layer antique inkjet brick has a strong sense of hierarchy and a good three-dimensional sense.

[0034] Preferably, the glaze layer is a matte glaze layer. In this embodiment, the surface of the multi-layer antique inkjet brick is an old inkjet matte, exuding a sense of fashion brought by retro, simple and elegant without losing its exquisiteness, and the size of the brick is visually expanded on the surface.

[0035] Preferably, in terms of mass percentage, the raw materials for preparing the bottom glaze layer include: 8% to 14% high temperature slurry, 4% to 8% zinc oxide, 13% to 15% zirconium silicate, 10% to 15% washed mud, 5% to 8% black mud powder, 35% to 40% red potassium sand, 8% to 10% burnt earth, 1% to 4% potassium feldspar, and 2% to 8% sodium soil. The formula of the bottom glaze layer is white glaze, which has a high whiteness and can effectively improve the color development effect of inkjet ink. The formula contains high temperature slurry, which can ensure the smoothness of the glaze surface and avoid defects such as ripples. It is characterized by high glaze hardness, high high temperature viscosity, large thermal expansion coefficient, low transparency, and a base for the middle glaze layer to ensure the overall whiteness.

[0036] Specifically, the content of high temperature paste and fired clay in the base glaze formula cannot be too much, otherwise the base glaze will have too high a high temperature viscosity, which is not conducive to the combination of body and glaze, and will cause defects such as raw fired glaze cracks. The content of zirconium silicate cannot be too little, because the base glaze is a cosmetic soil, and its function is to cover blemishes. Zirconium silicate can increase the whiteness of the base glaze, so that it covers the body and makes the ink color more vivid.

[0037] Specifically, the raw materials for preparing the high temperature slurry include, by mass percentage, 22% to 28% of waste materials, 15% to 20% of potassium feldspar, 13% to 18% of sodium feldspar, 8% to 12% of black mud powder, 8% to 12% of quartz, and 18% to 24% of kaolin. The waste materials may be used tailings or waste mud obtained after wastewater has been precipitated.

[0038] Preferably, the raw materials for preparing the glaze layer include, by mass percentage: 23% to 30% albite, 12% to 18% high-temperature potassium feldspar, 10% to 15% calcite, 5% to 8% burnt talc, 5% to 10% black mud, 10% to 12% burnt kaolin, 2% to 5% calcined zinc oxide, and 13% to 18% barium carbonate. The formula of the glaze layer is an improved matte glaze. The effect of conventional matte glaze is not ideal, which easily leads to unstable color development of blue-purple in inkjet printing. The improved matte glaze is adjusted by adding feldspar, which can make the blue tone turn green and stable, thereby promoting the product effect. In addition, the formula also contains a large amount of calcium and barium, which makes the glaze surface smooth and has strong anti-fouling ability. When forming a multi-layered glaze effect with the middle glaze layer, it will not hide dirt and is easy to clean.

[0039] In addition, the content of feldspar and calcite in matte glaze cannot be too much, otherwise its high-temperature viscosity will become low, and the fluidity will increase during the firing process, which will melt into the glossy glaze. Excessive content of feldspar and calcite will also cause the glossiness of matte glaze to be close to that of glossy glaze, which cannot produce contrast, seriously affecting the layering effect, and will also make the glossiness of the product too high and exceed the glossiness range required for antique tiles. Black mud and burnt earth are the main sources of aluminum oxide in matte glaze. If the aluminum oxide content is too little, the high-temperature viscosity will be too low, which will make the product glossier and make the glaze layer more fluid, and it will be easy to produce defects such as glaze flow during the firing process. Too much aluminum oxide will cause the firing temperature of the glaze slurry to be too high, greatly reducing the glossiness, failing to meet the glossiness requirements of antique tiles, and forming raw firing, which affects the color of the ink.

[0040] The third aspect of the present invention provides a method for preparing an antique inkjet brick, which is used to prepare the multi-layer antique inkjet brick described above, comprising the following steps:

[0041] S001. Applying white glaze on the body layer to form a bottom glaze layer;

[0042] S002. Applying a glossy glaze to form an intermediate glaze layer;

[0043] S003. Apply matte glaze and grind glaze by throwing point process to form a throwing point glaze layer;

[0044] S004. Inkjet to form an inkjet layer;

[0045] S005. Firing, the sintering temperature is 1225°C to 1230°C, and the firing cycle is 50 to 55 minutes.

[0046] Specifically, in S003, ink glazing is performed after the throwing point process, so that the top of the throwing point can be smooth and the gloss transition between the glossy glaze and the matte glaze is natural.

[0047] Preferably, the glaze slurry specific gravity of the white glaze is 1.33-1.35 g / cm 3 .

[0048] Preferably, the glaze slurry specific gravity of the glossy glaze is 1.33-1.35 g / cm 3 .

[0049] Preferably, the glaze slurry specific gravity of the matte glaze is 1.33-1.35 g / cm 3 The specific gravity of matte glaze cannot be too high. If the specific gravity of matte glaze is too high, the dots will be too protruding, and the combination of the glaze layer and the middle glaze layer will be unnatural, affecting the layering effect. The frequency of brushing dots cannot be too high. If the frequency of brushing dots is too high, the dots will be smaller, the surface effect will be more fragmented, and the effect will not change naturally.

[0050] In the present invention, by strictly controlling the specific gravity of each glaze slurry, it can be ensured that each glaze layer is tightly bonded, thereby avoiding precipitation and not affecting the inkjet effect.

[0051] Preferably, in the throwing-off process, a throwing-off cabinet is used for the throwing-off operation, the frequency of the throwing-off cabinet is 3 to 7 Hz, and the speed of the conveyor belt is 14 to 16 cm / s.

[0052] The three glazes required by the present invention do not need to be color-adjusted, and the pattern display is completed by inkjet technology. The three glazes can directly adjust the glaze slurry parameters and apply the glaze. The white glaze (used for the bottom glaze layer) needs to have a certain viscosity, otherwise it is easy to have spots, and the glazing must be uniform and smooth, otherwise it is easy to affect the glaze surface of the entire product. The same is true for the glossy glaze (used for the middle glaze layer); in the most critical spot-spraying process, the glaze slurry ratio of the matte glaze is 1.35g / cm 3 When firing, the product will have different colors due to the different coloring abilities of the middle glaze layer and the glaze layer. The color of the glossy glaze part is darker, and the color of the matte glaze part is lighter. It is matched with the inkjet pattern to create the effect of antique bricks.

[0053] Specifically, the preparation of the green body layer includes the following steps:

[0054] (1) Grinding raw materials: Grind each raw material and pass it through a 10-mesh sieve;

[0055] (2) Batching and ball milling: Prepare the raw materials according to the set ratio, transport the prepared powder to the ball mill through the batching machine, add water to the water content of the mixture to 18% by weight, and start the ball mill to grind to the calibrated fineness;

[0056] (3) Mud homogenization: put the mud of qualified fineness into the mud pool and stir it evenly;

[0057] (4) Spray drying: The homogenized slurry is pumped into a drying tower, and the atomizer atomizes the slurry into fine droplets, which are dried and dehydrated by hot air (400°C to 600°C) in the drying tower to form powder particles. The particles flow out through the discharge port, and the air with fine powder and water vapor is collected by a bag filter, and then discharged from the exhaust fan after dust removal in a water bath.

[0058] (5) Silo aging: The powder enters the silo through the conveying system and is placed for a suitable period of time to further homogenize the moisture content of the powder; the moisture content of the powder is 5.6% to 6.2%; the particle size distribution of the powder is <1% for 20 mesh and above, 15% to 25% for 20 to 40 mesh, 40% to 50% for 40 to 60 mesh, and 15% to 20% for 60 to 80 mesh;

[0059] (6) Powder molding: The powder is transported to the press for molding. When pressure is applied to the blank, the powder particles are squeezed by the pressure and begin to move and move closer to each other. The blank shrinks and the air is expelled to form a blank layer. The maximum pressure during pressing is 160 bar and the thickness of the blank layer is 10 mm.

[0060] Example 1

[0061] A multi-layer antique inkjet brick, the preparation method of which comprises the following steps:

[0062] S001. Applying white glaze on the body layer to form a bottom glaze layer;

[0063] The raw materials for preparing the white glaze include, by mass percentage: 14% high temperature slurry, 6% zinc oxide, 14% zirconium silicate, 10% washed mud, 6% black mud powder, 35% red potassium sand, 8% burnt earth, 4% potassium feldspar, and 3% sodium earth;

[0064] The specific gravity of white glaze is 1.35g / cm 3 , flow rate 19s, glaze layer 0.34mm;

[0065] S002. Applying a glossy glaze to form an intermediate glaze layer;

[0066] The raw materials for preparing the glossy glaze include, by weight percentage, 45% of high-temperature potassium feldspar, 2% of calcite, 5% of black mud, 15% of quartz, 23% of barium carbonate, 5% of raw kaolin, and 5% of zinc oxide; when preparing the glossy glaze, 0.4% of sodium tripolyphosphate and 1.6% of carboxymethyl cellulose need to be added in an amount of the total weight of the raw materials;

[0067] The glaze slurry density of glossy glaze is 1.35g / cm3, the flow rate is 20s, and the glaze layer is 0.22mm;

[0068] S003. Apply matte glaze and grind glaze by throwing point process to form a throwing point glaze layer;

[0069] The raw materials for preparing the matte glaze include, by mass percentage, 25% of albite, 15% of high-temperature potassium feldspar, 12% of calcite, 8% of burned talc, 10% of black mud, 12% of burned kaolin, 3% of calcined zinc oxide, and 15% of barium carbonate; when preparing the matte glaze, 0.4% of sodium tripolyphosphate and 1.6% of carboxymethyl cellulose need to be added in an amount of the total weight of the raw materials;

[0070] The glaze slurry density of matte glaze is 1.34g / cm 3 , flow rate 20s, frequency of the throwing cabinet is 5Hz, belt speed is 15cm / s;

[0071] S004. Inkjet to form an inkjet layer;

[0072] S005. Firing, the sintering temperature is 1230° C., and the sintering cycle is 50 minutes.

[0073] Example 2

[0074] A multi-layer antique inkjet brick, the preparation method of which is different from that of Example 1 in that:

[0075] The formula of white glaze is different. Calculated by mass percentage, the raw materials for preparing the white glaze include: 14% high-temperature slurry, 6% zinc oxide, 14% zirconium silicate, 10% washed mud, 6% black mud powder, 35% red potassium sand, 8% burnt earth, 4% potassium feldspar, and 3% sodium soil.

[0076] Example 3

[0077] A multi-layer antique inkjet brick, the preparation method of which is different from that of Example 1 in that:

[0078] The formula of the glossy glaze is different. According to the mass percentage, the raw materials for preparing the glossy glaze include: 42% high-temperature potassium feldspar, 3% calcite, 5% black mud, 15% quartz, 25% barium carbonate, 5% raw kaolin, and 5% zinc oxide;

[0079] The formula of matte glaze is different. Calculated by mass percentage, the raw materials for preparing the matte glaze include: 24% albite, 14% high-temperature potassium feldspar, 12% calcite, 8% burned talc, 10% black mud, 12% burned kaolin, 3% calcined zinc oxide, and 17% barium carbonate.

[0080] Comparative Example 1

[0081] A multi-layer antique inkjet brick, the preparation method of which is different from that of Example 1 in that:

[0082] The formula of matte glaze is different. Calculated by mass percentage, the raw materials for the preparation of matte glaze include: 27% albite, 16% high-temperature potassium feldspar, 12% calcite, 3% burned talc, 10% black mud, 12% burned kaolin, 3% calcined zinc oxide, and 17% barium carbonate.

[0083] Comparative Example 2

[0084] A multi-layer antique inkjet brick, the preparation method of which is different from that of Example 1 in that:

[0085] The process parameters are different. In this comparative example, the flow rate of the white glaze is 17s.

[0086] Comparative Example 3

[0087] A multi-layer antique inkjet brick, the preparation method of which is different from that of Example 1 in that:

[0088] The formula of matte glaze is different. Calculated by mass percentage, the raw materials for the preparation of matte glaze include: 23% albite, 14% high-temperature potassium feldspar, 17% calcite, 5% burned talc, 9% black mud, 12% burned kaolin, 3% calcined zinc oxide, and 17% barium carbonate.

[0089] The above examples and comparative examples were tested for various properties, and the results were as follows:

[0090]

[0091]

[0092] Figure 1 This is a real-life picture of Example 1. In the picture, the color of the ink is as expected, the glaze layer forms an uneven effect, and the multi-layered antique inkjet bricks have a strong sense of layering and a good three-dimensional effect.

[0093] Figure 2This is the actual picture of Comparative Example 1. In the picture, a large number of small bubbles appear on the glaze surface of the tile, and the glaze surface is uneven. The reason is that when the talc content of the matte glaze is too low, the fluidity of the glaze will be reduced. During the exhaust process of firing, the gas cannot break through the glaze to lift the glaze layer, boiling bubbles will appear, and many bulging small bumps will appear on the surface, which greatly damage the smoothness of the glaze.

[0094] Figure 3 This is a real-life picture of Comparative Example 2. In the picture, the ceramic tile has "glaze burst" after firing, and the glaze layer is damaged. The reason is that when the flow rate of the white glaze is too low, the bonding performance between the glaze layers is not good, resulting in a large number of bubbles gathering between the two layers of glaze during the exhaust process to form large bubbles, which eventually lead to glaze burst and damage the normal glaze surface.

[0095] In comparative example 3, the glossiness of the glaze is too high and the color is too dark. The reason is that when the calcite content of the matte glaze is too high, the firing temperature of the glaze layer will be reduced, resulting in an increase in the glossiness of the glaze, which exceeds the luminosity requirement of antique tiles.

[0096] It is understandable that those skilled in the art can make equivalent substitutions or changes based on the technical solution and inventive concept of the present invention, and all these changes or substitutions should fall within the protection scope of the claims attached to the present invention.

Claims

1. A glossy glaze, characterized in that: Calculated by mass percentage, the raw materials for its preparation include: 40% to 46% of high-temperature potassium feldspar, 2% to 5% of calcite, 3% to 8% of black mud, 13% to 18% of quartz, 20% to 26% of barium carbonate, 3% to 8% of raw kaolin, and 3% to 8% of zinc oxide.

2. A multi-layer antique inkjet brick, characterized in that: It comprises a body layer, a bottom glaze layer, an intermediate glaze layer, a throwing glaze layer and an inkjet layer which are arranged in sequence; the intermediate glaze layer is made of the glossy glaze according to claim 1.

3. The multi-layer antique inkjet brick according to claim 2 is characterized in that: Measured by mass percentage, the raw materials for preparing the base glaze layer include: 8% to 14% high-temperature slurry, 4% to 8% zinc oxide, 13% to 15% zirconium silicate, 10% to 15% washed mud, 5% to 8% black mud powder, 35% to 40% red potassium sand, 8% to 10% burnt earth, 1% to 4% potassium feldspar, and 2% to 8% sodium soil.

4. The multi-layer antique inkjet brick according to claim 3 is characterized in that: Calculated by mass percentage, the raw materials for preparing the high-temperature slurry include: 22% to 28% of waste materials, 15% to 20% of potassium feldspar, 13% to 18% of sodium feldspar, 8% to 12% of black mud powder, 8% to 12% of quartz, and 18% to 24% of kaolin.

5. The multi-layer antique inkjet brick according to claim 2 is characterized in that: Calculated by mass percentage, the raw materials for preparing the glaze layer include: 23% to 30% of albite, 12% to 18% of high-temperature potassium feldspar, 10% to 15% of calcite, 5% to 8% of burned talc, 5% to 10% of black mud, 10% to 12% of burned kaolin, 2% to 5% of calcined zinc oxide, and 13% to 18% of barium carbonate.

6. A method for preparing antique inkjet bricks, characterized in that: The method for preparing the multi-layer antique inkjet brick according to any one of claims 2 to 5 comprises the following steps: S001. Applying white glaze on the body layer to form a bottom glaze layer; S002. Applying a glossy glaze to form an intermediate glaze layer; S003. Apply matte glaze and grind glaze by throwing point process to form a throwing point glaze layer; S004. Inkjet to form an inkjet layer; S005. Firing, the sintering temperature is 1225°C to 1230°C, and the firing cycle is 50 to 55 minutes.

7. The method for preparing antique inkjet bricks according to claim 6, characterized in that: The specific gravity of the white glaze slurry is 1.33-1.35 g / cm 3 ; The flow rate of the white glaze is 19 to 21 seconds; the flow rate of the glossy glaze is 19 to 21 seconds; the flow rate of the matte glaze is 19 to 21 seconds.

8. The method for preparing antique inkjet bricks according to claim 6, characterized in that: The specific gravity of the glaze slurry of the glossy glaze is 1.33-1.35 g / cm 3 .

9. The method for preparing antique inkjet bricks according to claim 6, characterized in that: The glaze slurry specific gravity of the matte glaze is 1.33-1.35 g / cm 3 .

10. The method for preparing antique inkjet bricks according to claim 6, characterized in that: In the throwing-off process, a throwing-off cabinet is used for the throwing-off operation, the frequency of the throwing-off cabinet is 3-7 Hz, and the speed of the conveyor belt is 14-16 cm / s.

Citation Information

Patent Citations

  • Dry glaze for pasedo-classic glazed tile

    CN101045647A

  • Ink-jet brick and production process thereof

    CN112340991A

  • Stain-resistant glazed tile and production process thereof

    CN112456967A

  • Dry-particle semi-polished brick preparation process

    CN113698190A

  • Archaized brick with antiskid effect and preparation method of archaized brick

    CN114349543A

Cited By

  • Method for preparing bright-spot matt fancy glaze from waste porcelain powder

    CN120309174A