Glass ceramic, chemically strengthened glass ceramic and application of chemically strengthened glass ceramic

By optimizing the composition of the glass-ceramic and chemical strengthening treatment, and increasing the content of lithium disilicate crystalline phase, a glass-ceramic with high stress level and excellent deformation resistance was prepared, solving the problem of easy damage to cover glass and improving the deformation resistance and display stability of electronic devices.

CN118930055AActive Publication Date: 2024-11-12CHONGQING AUREAVIA HI TECH GLASS CO LTD

Patent Information

Application Number
CN202410156362.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-02-02
Publication Date
2024-11-12
Estimated Expiration
2044-02-02

AI Technical Summary

Technical Problem

When existing microcrystalline glass is used as cover glass in electronic devices, the inner screen is prone to failure due to compression or impact. Furthermore, the existing microcrystalline glass has insufficient resistance to deformation and cannot effectively protect the inner screen.

Method used

By optimizing the composition and structure of the glass-ceramic, increasing the content of lithium disilicate crystalline phase, and through chemical strengthening treatment, a glass-ceramic with high stress level and excellent deformation resistance was prepared. The interlocking structure of lithium disilicate crystals was used to hinder crack propagation.

Benefits of technology

The improved mechanical strength and optical properties of microcrystalline glass enable it to effectively resist external pressure or impact, reduce the possibility of failure of the inner glass screen, and ensure the stability and display effect of electronic devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930055A_ABST
    Figure CN118930055A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of glass ceramics, and particularly relates to glass ceramics, chemically strengthened glass ceramics and application of the chemically strengthened glass ceramics, the glass ceramics comprise a main crystalline phase lithium disilicate crystalline phase and have specific ranges of the content of each oxide, and the composition of the glass ceramics meets the condition that SiO2 / Li2O is larger than or equal to 2.00 and smaller than or equal to 2.40 according to the content expressed by the mole percent of each oxide in the composition of the glass ceramics. The microcrystalline glass provided by the invention has high intrinsic strength and excellent optical performance, and the chemically strengthened microcrystalline glass with high stress level and excellent deformation resistance can be prepared through chemical strengthening.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of microcrystalline glass technology, and specifically relates to a microcrystalline glass with excellent deformation resistance, chemically strengthened microcrystalline glass and applications thereof. Background Art

[0002] With the advent of the smart era, portable electronic devices such as mobile phones, tablets, and watches have become an indispensable part of daily life, and most of their damage is caused by screen shattering. With the introduction of microcrystalline glass such as "Kunlun Glass", "Super Ceramic Crystal", and "Titan Glass", the probability of cover glass shattering has been greatly reduced. However, the problem of glass inner screen failure needs to be further improved. If the inner screen fails, touch failure, display abnormality, screen damage and other phenomena are likely to occur. Especially driven by the market demand for larger and thinner electronic devices, the thickness of cover glass is getting thinner and thinner. When the cover glass is squeezed or impacted and deformed, it will squeeze the inner screen of the glass, which may cause the inner screen to fail. Therefore, in order to better improve the problem of glass inner screen failure caused by impact on the cover glass, it is urgent to develop a cover glass with excellent deformation resistance. Summary of the invention

[0003] As a solid material containing microcrystalline phase and glass phase, glass-ceramics has obvious advantages in overall strength performance over conventional glass because of the large number of nano-sized tiny crystals it contains, which can hinder the expansion of microcracks. Among the existing glass-ceramics, glass-ceramics with lithium disilicate as the main crystal phase has great application potential as cover glass in electronic products.

[0004] The lithium disilicate (Li2Si2O5) crystal phase is an orthorhombic crystal based on the [Si2O5] tetrahedral array, and the crystal shape is flat or plate-like. Inside the glass-ceramic, the lithium disilicate crystals are randomly oriented interlocking microstructures, forcing the crack path to be distorted when passing through the crystal, thereby preventing the crack from expanding and improving the strength and fracture toughness of the glass-ceramic. At the same time, the refractive index of lithium disilicate crystals is close to that of the glass matrix (e.g., the base glass for preparing glass-ceramics), making it an ideal crystal phase for preparing highly transparent glass-ceramics.

[0005] In view of this, the purpose of this application is to provide a microcrystalline glass with high strength and excellent optical properties, with lithium disilicate as the main crystalline phase. The microcrystalline glass can be prepared by chemical strengthening to obtain chemically strengthened microcrystalline glass with high stress level, excellent deformation resistance and high mechanical strength.

[0006] In order to achieve the above objectives, this application provides the following technical solutions:

[0007] 1. A glass-ceramic, wherein the glass-ceramic contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the glass-ceramic;

[0008] The composition of the glass-ceramics includes, in terms of molar percentage of oxides:

[0009] SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol% , Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;

[0010] The composition of the glass-ceramics satisfies the following conditions: 2.00≤SiO2 / Li2O≤2.40, preferably 2.00≤SiO2 / Li2O≤2.30, and more preferably 2.02≤SiO2 / Li2O≤2.20. By optimizing the glass formula, such as using a higher content of zirconium and a lower content of aluminum under a higher content of lithium, and making the various components satisfy a specific content relationship and interact with each other, on the one hand, it is beneficial to ensure the precipitation of the desired content of lithium disilicate crystal phase and limit the precipitation of other crystal phases (such as petalite crystal phase), thereby helping to ensure that the glass-ceramics with high intrinsic strength and excellent optical properties and with lithium disilicate as the main crystal phase are obtained. On the other hand, it is beneficial to ensure that the glass-ceramics meets the specific composition and structure, thereby ensuring that after chemical strengthening, chemically strengthened glass-ceramics with high stress level and excellent deformation resistance are prepared.

[0011] 2. The glass-ceramics according to technical solution 1, wherein the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, further satisfies:

[0012] 0.90≤SiO2+Li2O≤0.96, preferably, 0.90≤SiO2+Li2O≤0.95; and / or,

[0013] Al2O3 / SiO2≤0.030. By adjusting the components to meet the specific content relationship, it is beneficial to ensure the formation of the desired crystal phase structure, and it is also beneficial to improve the stress level generated by the microcrystalline glass after chemical strengthening, which is beneficial to ensure that the microcrystalline glass obtains high mechanical strength and excellent deformation resistance.

[0014] 3. The glass-ceramics according to technical solution 1 or 2, wherein the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, further satisfies:

[0015] 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50, preferably, 0.32≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.20, more preferably, 0.36≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.10;

[0016] and / or,

[0017] 0.10≤ZrO2 / (100%-3×Li2O)≤0.60, preferably, 0.12≤ZrO2 / (100%-3×Li2O)≤0.52, more preferably, 0.16≤ZrO2 / (100%-3×Li2O)≤0.50;

[0018] and / or,

[0019] 0.034≤ZrO2 / SiO2≤0.100, preferably, 0.035≤ZrO2 / SiO2≤0.095, more preferably, 0.055≤ZrO2 / SiO2≤0.095. By adjusting the components to meet the specific content relationship, it is beneficial to exert the strengthening or toughening effect of each component and the interaction of each component, thereby ensuring the high intrinsic strength of the microcrystalline glass and the high stress level after strengthening, which is beneficial to ensure that the microcrystalline glass obtains high mechanical strength performance and excellent deformation resistance.

[0020] 4. The glass-ceramics according to any one of technical solutions 1 to 3, wherein the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, further satisfies:

[0021] CaO+Al2O3≤0.065, preferably, CaO+Al2O3≤0.055, more preferably, CaO+Al2O3≤0.050;

[0022] and / or,

[0023] (CaO+Al2O3) / Li2O≤0.25, preferably, (CaO+Al2O3) / Li2O≤0.20, more preferably, (CaO+Al2O3) / Li2O≤0.14. By adjusting the components to meet the specific content relationship, it is beneficial to avoid affecting the crystallization of the microcrystalline glass while exerting the effects of the reinforcement of each component, thereby ensuring that the microcrystalline glass achieves the desired crystalline phase structure, and further helps to ensure that the microcrystalline glass obtains high mechanical strength performance and excellent deformation resistance.

[0024] 5. The glass-ceramics according to any one of technical solutions 1 to 4, wherein the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, further satisfies:

[0025] 0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40, preferably, 0.14≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.16, more preferably, 0.50≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤3.00;

[0026] and / or,

[0027] Na2O / SiO2≤0.05, preferably, Na2O / SiO2≤0.04, more preferably, Na2O / SiO2≤0.02. By adjusting the components to meet the specific content relationship, it is beneficial to better play the role of each component, to make the microcrystalline glass obtain high intrinsic strength and excellent optical properties, and to make the microcrystalline glass obtain high stress level and excellent deformation resistance after chemical strengthening.

[0028] 6. The glass-ceramic according to any one of technical solutions 1 to 5, wherein, in terms of molar percentage of oxides, the glass-ceramic comprises:

[0029] The content of SiO2 is 60.00mol%-65.00mol%, preferably the content of SiO2 is 60.50mol%-64.00mol%; and / or,

[0030] The content of Li2O is 28.00mol%-31.00mol%, preferably the content of Li2O is 29.00mol%-30.50mol%; and / or,

[0031] The content of ZrO2 is 3.20mol%-6.00mol%, preferably the content of ZrO2 is 4.00mol%-6.00mol%; and / or,

[0032] The content of P2O5 is 1.50mol%-3.00mol%, preferably the content of P2O5 is 1.50mol%-2.50mol%; and / or,

[0033] The content of Na2O is 0.00mol%-1.00mol%, preferably the content of Na2O is 0.00mol%-0.50mol%; and / or,

[0034] The content of CaO is 0.00 mol%-4.00 mol%, preferably 0.00 mol%-2.50 mol%. By adjusting the composition of the microcrystalline glass, the microcrystalline glass can obtain high mechanical strength and excellent anti-deformation ability.

[0035] 7. The glass-ceramic according to any one of technical solutions 1 to 6, wherein the composition of the glass-ceramic further comprises, in terms of the molar percentage of oxides: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%. The selective addition of an appropriate amount of Y2O3, La2O3 or Ta2O5 helps to increase the density of the glass-ceramic and increase its Young's modulus, but may also increase the refractive index of the glass-ceramic and reduce the optical properties of the glass-ceramic.

[0036] 8. A glass-ceramic according to any one of technical solutions 1-7, wherein, in terms of molar percentage of oxides, the sum of the molar percentage contents of Na2O and K2O in the glass-ceramic is less than 1.00 mol%.

[0037] 9. The glass-ceramic according to any one of technical solutions 1 to 8, wherein the density of the glass-ceramic is ρ≥2.50 g / cm 3 Preferably, the density ρ of the microcrystalline glass is 2.50 g / cm 3 ~2.75g / cm 3 ; and / or, the refractive index of the microcrystalline glass is ≤1.60. Microcrystalline glass satisfying this density and / or refractive index can ensure high intrinsic strength and excellent optical properties.

[0038] 10. The glass-ceramics according to any one of technical solutions 1 to 9, wherein the crystallinity of the glass-ceramics is 30.00wt%-90.00wt%, preferably, the crystallinity is 50.00wt%-90.00wt%, and the crystallinity is 65.00wt%-90.00wt%;

[0039] and / or,

[0040] In the microcrystalline glass, the average crystal size is ≤100nm, preferably, the average crystal size is ≤50nm, and more preferably, the average crystal size is 15nm to 45nm. A higher content of crystalline phase is beneficial to improving the mechanical strength of the microcrystalline glass, and meeting the smaller average crystal size is beneficial to ensuring that the microcrystalline glass has excellent optical properties.

[0041] 11. The glass-ceramic according to any one of technical solutions 1 to 10, wherein the Young's modulus of the glass-ceramic is ≥ 100.00 GPa, preferably, the Young's modulus of the glass-ceramic is ≥ 110.00 GPa, and more preferably, the Young's modulus of the glass-ceramic is 114 GPa to 130 GPa. A higher Young's modulus indicates that the glass-ceramic has a higher intrinsic strength, which is conducive to obtaining higher mechanical strength and excellent deformation resistance.

[0042] 12. The glass-ceramic according to any one of technical solutions 1 to 11, wherein at a thickness of 0.5 mm, the b value of the glass-ceramic is ≤1.0, preferably ≤0.8; and / or

[0043] The microcrystalline glass is transparent in the visible light range; at a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the microcrystalline glass is ≥ 85.00%, preferably, the transmittance of the microcrystalline glass is ≥ 90.00%. Microcrystalline glass that meets the optical b value and / or transmittance can ensure better optical performance and display effect, and is suitable for use in display screens that require display effects.

[0044] 13. The glass-ceramic according to any one of technical solutions 1 to 12, wherein the expansion softening point of the glass-ceramic is 750° C. to 850° C., preferably, the expansion softening point of the glass-ceramic is 750° C. to 830° C. A suitable expansion softening point is conducive to 3D hot bending of the glass-ceramic to obtain a 3D curved glass-ceramic with high strength.

[0045] 14. A chemically strengthened glass-ceramic, wherein the composition at the center of the chemically strengthened glass-ceramic is the same as the composition of the glass-ceramic described in any one of Technical Solutions 1-13, and the chemically strengthened glass-ceramic includes a compressive stress layer region extending from the surface of the chemically strengthened glass-ceramic to the compression depth, and has tensile stress inside the chemically strengthened glass-ceramic.

[0046] 15. The chemically strengthened glass-ceramics according to technical solution 14, wherein the chemically strengthened glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; and the composition at the center of the chemically strengthened glass-ceramics, in terms of molar percentage of oxides, includes: SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-3.00mol%, mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.0 0mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;

[0047] The composition at the center of the chemically strengthened glass-ceramics, expressed in terms of the content as a molar percentage of oxides, satisfies: 2.00≤SiO2 / Li2O≤2.40, preferably, 2.00≤SiO2 / Li2O≤2.30, and more preferably, 2.02≤SiO2 / Li2O≤2.20.

[0048] 16. The chemically strengthened glass-ceramics according to claim 14 or 15, wherein the composition at the center of the chemically strengthened glass-ceramics, expressed in terms of the content expressed in molar percentage of oxides, further satisfies:

[0049] 0.90≤SiO2+Li2O≤0.96; and / or,

[0050] Al2O3 / SiO2≤0.030; and / or,

[0051] 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50; and / or,

[0052] 0.10≤ZrO2 / (100%-3×Li2O)≤0.60; and / or,

[0053] 0.034≤ZrO2 / SiO2≤0.100; and / or,

[0054] CaO+Al2O3≤0.065; and / or,

[0055] (CaO+Al2O3) / Li2O≤0.25; and / or,

[0056] 0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40; and / or,

[0057] Na2O / SiO2≤0.05.

[0058] 17. The chemically strengthened glass-ceramics according to any one of technical solutions 14 to 16, wherein the composition at the center of the chemically strengthened glass-ceramics, measured in molar percentage of oxides, comprises:

[0059] The content of SiO2 is 60.00mol%-65.00mol%, preferably the content of SiO2 is 60.50mol%-64.00mol%; and / or, the content of Li2O is 28.00mol%-31.00mol%, preferably the content of Li2O is 29.00mol%~30.50mol%; and / or, the content of ZrO2 is 3.20mol%-6.00mol%, preferably the content of ZrO2 is 4.00mol%~6.00mol% 1%; and / or, the content of P2O5 is 1.50mol%-3.00mol%, preferably the content of P2O5 is 1.50mol%~2.50mol%; and / or, the content of Na2O is 0.00mol%-1.00mol%, preferably the content of Na2O is 0.00mol%~0.50mol%; and / or, the content of CaO is 0.00mol%-4.00mol%, preferably the content of CaO is 0.00mol%-2.50mol%.

[0060] 18. A chemically strengthened glass-ceramic according to any one of technical solutions 14-17, wherein the composition at the center of the chemically strengthened glass-ceramic, measured in molar percentage of oxides, further includes: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

[0061] 19. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 18, wherein the chemically strengthened glass-ceramic has a DOL_0 of 0.18t-0.25t, preferably, the chemically strengthened glass-ceramic has a DOL_0 of 0.20t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramic. The DOL_0 of the chemically strengthened glass-ceramic is within the above range, indicating that the chemically strengthened glass-ceramic has a high depth of the compressive stress layer, which is more conducive to offsetting the energy driving the crack extension, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0062] 20. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 19, wherein the chemically strengthened glass-ceramic has a |CT_AV| of 85MPa-200MPa, preferably, the chemically strengthened glass-ceramic has a |CT_AV| of 90MPa-200MPa, and more preferably, the chemically strengthened glass-ceramic has a |CT_AV| of 130MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress. The |CT_AV| of the chemically strengthened glass-ceramic is within the above range, indicating that the chemically strengthened glass-ceramic has a higher tensile stress level, reflecting that it has a higher surface stress level, and the higher the surface compressive stress level, the more residual energy of the drop collision can be offset, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0063] 21. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 20, wherein the chemically strengthened glass-ceramic has a CT_LD of 50000MPa / mm-100000MPa / mm, preferably, the chemically strengthened glass-ceramic has a CT_LD of 55000MPa / mm-100000MPa / mm, and more preferably, the chemically strengthened glass-ceramic has a CT_LD of 65000MPa / mm-100000MPa / mm, where CT_LD is the tensile stress linear density. The range of CT_LD of the chemically strengthened glass-ceramic is within the above range, indicating that the tensile stress stored inside the chemically strengthened glass-ceramic is relatively dense, indicating that the chemically strengthened glass-ceramic has a higher surface stress level, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0064] 22. The chemically strengthened glass-ceramic according to any one of technical solutions 14 to 21, wherein the chemically strengthened glass-ceramic has a |CT_CV| of 120MPa-320MPa, preferably, the chemically strengthened glass-ceramic has a |CT_CV| of 135MPa-300MPa, and more preferably, the chemically strengthened glass-ceramic has a |CT_CV| of 160MPa-300MPa. The range of |CT_CV| of the chemically strengthened glass-ceramic is within the above range, indicating that the chemically strengthened glass-ceramic has a higher tensile stress level, reflecting that it has a higher surface stress level, and the higher surface compressive stress level can offset more residual energy of falling collision, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0065] 23. The chemically strengthened glass-ceramics according to any one of technical solutions 14 to 22, wherein the Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 680 kgf / mm 2 Preferably, the Vickers hardness of the chemically strengthened glass-ceramics is 700 kgf / mm2 ~800kgf / mm 2 The Vickers hardness of the chemically strengthened glass-ceramics is within the above range, indicating that the chemically strengthened glass-ceramics has high hardness, thereby ensuring that it has excellent mechanical properties.

[0066] 24. The chemically strengthened glass-ceramic according to any one of technical solutions 14-23, wherein, at a thickness of 0.5 mm, a 10 mm diameter round head metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened glass-ceramic, and when the center of the main surface of the chemically strengthened glass-ceramic is subjected to a 10 kgf load, the deformation of the stress position of the chemically strengthened glass-ceramic in the stress direction is ≤ 0.850 mm. The smaller the deformation of the chemically strengthened glass-ceramic after being squeezed, the better its anti-deformation ability is. When it is used as the cover glass of a display screen, the smaller the deformation after being squeezed or impacted, the smaller the probability of contacting the inner screen of the glass is, which is conducive to improving the problem of failure of the inner screen of the glass caused by the impact of the cover glass.

[0067] 25. The chemically strengthened glass-ceramic according to any one of technical solutions 14-24, wherein, at a thickness of 0.5 mm, a 10 mm diameter round head metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened glass-ceramic, and when the center of the main surface of the chemically strengthened glass-ceramic undergoes a deformation of 0.400 mm along the force direction, the load borne by the center of the main surface of the chemically strengthened glass-ceramic is ≥ 30 N. When a certain amount of deformation occurs, the greater the load that the chemically strengthened glass-ceramic can withstand, the greater the load that can be offset by the deformation when the chemically strengthened glass-ceramic is subjected to extrusion or impact, so when the deformation contacts the inner screen of the glass, the extrusion or impact load borne by the inner screen of the glass will be smaller, and the possibility of failure of the inner screen of the glass will be reduced. Using chemically strengthened glass-ceramic that can withstand or offset a large load as the cover glass is conducive to improving the problem of failure of the inner screen of the glass caused by impact or extrusion of the cover glass. .

[0068] 26. A glass device, wherein the glass device comprises the microcrystalline glass as described in any one of Technical Solutions 1 to 13 or comprises the chemically strengthened microcrystalline glass as described in any one of Technical Solutions 14 to 25.

[0069] 27. An electronic device, wherein the electronic device comprises the microcrystalline glass as described in any one of Technical Solutions 1-13 or comprises the chemically strengthened microcrystalline glass as described in any one of Technical Solutions 14-25.

[0070] Beneficial effects:

[0071] In the present application, by making the microcrystalline glass containing lithium disilicate as the main crystalline phase meet specific composition and structure, especially meet the oxide content and specific oxide content relationship under specific conditions, it is not only ensured that the microcrystalline glass has high intrinsic strength and excellent optical properties, but also ensured that the microcrystalline glass can be prepared by chemical strengthening to obtain chemically strengthened microcrystalline glass with high stress level (such as high CT_LD, |CT_AV|, DOL_0, etc.) and excellent deformation resistance. The chemically strengthened microcrystalline glass made by the microcrystalline glass of the present application, as the cover glass of the electronic device display screen, can better overcome the problem in the prior art that the inner screen of the glass is easily failed due to deformation and extrusion of the cover glass. BRIEF DESCRIPTION OF THE DRAWINGS

[0072] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0073] Figure 1 This is the DSC curve of the substrate glass of Example 3.

[0074] Figure 2 This is the XRD spectrum of the microcrystalline glass of Example 3.

[0075] Figure 3 This is a transmittance curve of the microcrystalline glass of Example 3.

[0076] Figure 4 This is a load-deformation curve of the chemically strengthened microcrystalline glass of Example 3.

[0077] Figure 5 This is the load-deformation curve of the chemically strengthened microcrystalline glass of comparative example 3. DETAILED DESCRIPTION

[0078] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they can be included or not (or can be included or not).

[0079] Glossary and test methods:

[0080] Base glass: glass that has not been subjected to nucleation, crystallization or strengthening treatment.

[0081] Glass-ceramics: also known as glass ceramics, is a type of solid composite material that contains both a glass phase and a crystal phase (also called a microcrystalline phase or a crystalline phase) and is prepared by targeted and controlled crystallization of the base glass.

[0082] Chemically strengthened glass-ceramics: refers to the solid composite material obtained after chemical strengthening treatment of glass-ceramics. During high-temperature chemical strengthening treatment, the alkali metal ions with large ionic radius (such as potassium ions or sodium ions) in the molten salt bath will replace the alkali metal ions with small ionic radius (such as sodium ions or lithium ions) in the glass-ceramics, thereby generating an exchange ion volume difference and generating compressive stress (also called compression stress) on the surface of the glass-ceramics.

[0083] Main crystalline phase or major crystalline phase: refers to a crystalline phase having a higher weight content than other crystalline phases present in the microcrystalline glass.

[0084] Main surface: refers to the surface with the largest surface area in the glass brick or glass sheet, such as the upper and lower surfaces of the cover glass.

[0085] Crystallinity: refers to the percentage of the total mass of the crystalline phase or crystals in the microcrystalline glass to the mass of the microcrystalline glass, or also called the total content of the crystalline phase in the microcrystalline glass.

[0086] Refractive index: The refractive index refers to the ratio of the speed of light in a vacuum to the speed of light in the medium.

[0087] Transmittance: When light of a certain wavelength is irradiated onto the glass surface, the light will be reflected, absorbed and transmitted. The ratio of the intensity of the transmitted part to the intensity of the incident light is the transmittance.

[0088] SOC: Photoelastic coefficient. Photoelasticity mainly refers to the phenomenon of anisotropy and birefringence of transparent materials after being subjected to force. By measuring the photoelastic coefficient and birefringence, the value of the residual stress (in MPa) inside the material can be obtained.

[0089] CT_LD: refers to the tensile stress linear density, measured in MPa / mm. It should be understood that after the glass-ceramics is placed in a molten salt bath for ion exchange, a compressive stress layer (or also called a compressive stress layer) will be formed on the surface of the glass-ceramics, and a tensile stress layer (or also called a tensile stress layer) will be formed inside the glass-ceramics. Exemplarily, during chemical strengthening, alkali metal ions with a large radius in the molten salt bath are ion exchanged with alkali metal ions with a small radius in the glass-ceramics, thereby forming a compressive stress layer on the surface of the glass-ceramics and a tensile stress layer inside the glass-ceramics. In this application, CT_LD is calculated by the following formula:

[0090]

[0091] Wherein, t is the thickness of the chemically strengthened glass-ceramics, in mm; DOL 0 is the depth of the compressive stress layer of the chemically strengthened glass-ceramics, in μm; |CT_AV| is the absolute value of the average tensile stress of the chemically strengthened glass-ceramics, in MPa. It should be understood that in the calculation formula of the tensile stress linear density, the data is substituted into the calculation according to the above unit requirements, and the calculation result is obtained, and the unit does not participate in the calculation.

[0092] |CT_CV|: refers to the absolute value of the maximum tensile stress, in MPa, specifically the absolute value of the maximum value of all tensile stresses in the tensile stress layer, obtained by testing with the SLP-2000 stress meter.

[0093] |CT_AV|: refers to the absolute value of the average tensile stress, in MPa, specifically the absolute value of the average value of all tensile stresses in the tensile stress layer, obtained by testing with the SLP-2000 stress meter.

[0094] DOL_0: refers to the depth of the compressive stress layer, or the depth of the compressive stress layer, specifically the distance from any main surface of the chemically strengthened microcrystalline glass to the position close to the surface where the compressive stress is zero, obtained by testing with the SLP-2000 stress meter.

[0095] b value: used to characterize the yellow-blue value of a material. The optical b value in the present invention is the b value of transmitted light, and a positive optical b value indicates that the material is blue.

[0096] Vickers hardness: Vickers hardness refers to a standard for expressing the hardness of materials proposed by Robert L. Smith and George E. Sandland of the United Kingdom at Vickers Ltd in 1921.

[0097] Upper limit temperature of crystallization: The upper limit temperature of crystallization refers to the highest temperature at which the substrate glass produces crystallization. Above this temperature, the substrate glass will not precipitate crystals.

[0098] Thickness of glass: measured by micrometer. It should be understood that in the thickness direction, the degree of ion exchange changes gradually from the surface to the center, and the total Na-K and / or Li-Na exchange amount generally does not exceed 1.5% of the total mass of the sample, and the difference in ion radius is at the pm level, so the expansion effect in the thickness direction is extremely slight, and it can be approximately considered that the thickness has basically not changed. That is, the thickness change of microcrystalline glass before and after chemical strengthening is very small and can be ignored.

[0099] Glass sheet size specification measurement: tested using a two-dimensional measuring machine (instrument model: Miyu MY-YXCL-4030).

[0100] XRD test: The glass-ceramics or chemically strengthened glass-ceramics of the present application is crushed and ground into a sample with a particle size of less than 75 μm, and the ground sample is tested using an X-ray diffractometer to obtain an XRD diffraction peak curve and XRD diffraction data. The X-ray diffractometer used in the present application is Shimadzu XRD-6100, the incident angle range used in the test is 2θ=10°-60°, the scanning speed is 0.2° / min, the operating voltage is 40 kV, and the operating current is 30 mA.

[0101] Determination of crystalline phase: XRD diffraction data were analyzed using Jade software (JADE Standard 8.6) to determine the crystalline phase in the sample.

[0102] Determination of crystallinity: The XRD test results (RAW format) are imported into the X-ray diffraction data Rietveld refinement software Jade for fitting and calculation to determine the crystallinity of the sample. Specifically, the ratio of the fitted crystalline phase peak area to the fitted total peak area is recorded as the crystallinity of the sample.

[0103] Determination of average crystal size: Using the result data obtained from the XRD test, the average crystal size of the sample can be calculated according to the Scherrer formula D = Kλ / (βcosθ). Wherein, λ is the X-ray wavelength, λ = 0.154056nm, β is the half-height width of the diffraction peak, K = 0.89, and θ is the Bragg diffraction angle. Specifically, the RAW format file output by the XRD instrument is curve fitted in the Jade software, and Jade outputs a fitting report. According to the angle 2θ value and PeakFWHM value corresponding to each diffraction peak in the fitting report, the Peak FWHM value is converted into radians: β = (FWHM / 180×3.14), and the crystal size of each diffraction peak is calculated by the Scherrer formula D = Kλ / (βcosθ) and then averaged to obtain the average crystal size in the sample.

[0104] Test of transmittance and optical b-value: With reference to the national standard "GB / T 7962.12-2010 Test method for colorless optical glass Part 12: Spectral transmittance", a haze meter is used to test the transmittance and optical b-value of the microcrystalline glass of this application. Specifically, a haze meter is used to test the transmittance and optical b-value of 5 microcrystalline glass pieces of the same batch for light of different wavelengths. The average value of the optical b-values ​​measured for the 5 microcrystalline glass pieces is taken as the optical b-value result of the microcrystalline glass. The average value of the transmittance measured for the 5 microcrystalline glass pieces at a wavelength of 550nm is taken as the transmittance result of the microcrystalline glass at a wavelength of 550nm. Among them, the haze meter used in the test of this application is the Konica Minolta spectrophotometer CM-3600A from Japan, the light receiving optical system is transmission, the spectroscopic method is a plane reflective grating, the wavelength range is 360nm-740nm, the wavelength spacing is 10nm, the illumination light source is a pulsed xenon lamp X4, the ambient temperature of the instrument is 24°C, and the air humidity is 40%.

[0105] Density: This application uses the electronic density balance SD-200L of Japan ALFAMIRAGE to test the density of microcrystalline glass.

[0106] Refractive index: This application uses a WYA-2WAJ Abbe refractometer to measure the refractive index of microcrystalline glass.

[0107] Expansion softening point temperature: The sample is made into a cylinder with a diameter of 5.5 mm and a length of 20 mm. The sample is tested using a thermal expansion instrument LINSEIS L75VD1000. The test outputs a thermal expansion coefficient test curve. The corresponding temperature when the curve begins to decrease with increasing temperature is recorded as the expansion softening point temperature of the sample.

[0108] Young's modulus: The UMS-100 ultrasonic material characterization system was used to test the Young's modulus of glass-ceramics by sound waves.

[0109] Crystallization upper limit temperature: Break the substrate glass into small pieces, then put them into the long quartz tank and fill them up. Set the temperature range of the gradient furnace model JKZC-XJY01, such as the temperature range of 1050℃-1225℃, and take at least 6 temperature points from high to low in each temperature range. After the gradient furnace reaches the preset temperature range, put the long quartz tank with the sample into the gradient furnace, so that the 6 temperature points correspond to the glass samples at 6 positions in the long quartz tank, and place the long quartz tank in the gradient furnace at a constant temperature for 60-70 minutes, and then take out the long quartz tank. Use a microscope or magnifying glass to observe the glass samples at different positions in the long quartz tank. If the glass sample is devitrified or foggy, it is determined that the glass sample at that location is crystallized. If the glass sample is completely transparent, it is determined that the glass sample at that location is not crystallized. The crystallization upper limit temperature range is between the temperature point corresponding to the completely transparent sample and the temperature point corresponding to the adjacent devitrified or fogged sample. The average value of the two temperature points is recorded as the crystallization upper limit temperature. If all or none of the glass samples in the long quartz tank crystallize within the temperature range set by the gradient furnace, the temperature range of the gradient furnace is reset to measure the crystallization upper limit temperature of the glass sample.

[0110] Vickers hardness test: The chemically strengthened microcrystalline glass is made into a small piece with a length, width and thickness of 50mm×50mm×0.5mm, and a glass sample with a clean surface and no visible scratches, pits, cracks and other damage is selected as a test sample, and then the Vickers hardness is measured using a Vickers hardness tester. The Vickers hardness tester used in the test of the present invention is a digital display small load Vickers hardness tester model VTD405 of Beijing Kewei Technology Co., Ltd. Test conditions: load 300gf, load time 10s, the effectiveness of the indentation complies with the standard of "GB / T 37900-2019 Ultra-thin glass hardness and fracture toughness test method small load Vickers hardness indentation method". Select 3 different positions on the surface of the same test sample for measurement, and take the average of the 3 measurement results, which is recorded as the Vickers hardness result of the test sample.

[0111] Synchronous thermal analysis test: After the substrate glass is crushed, ground and sieved through 200 meshes to obtain a sample, then weigh about 20 mg of the sample, use a differential thermal analyzer, and heat from room temperature to 1100°C at a heating rate of 10°C / min under a nitrogen atmosphere to obtain the DSC test curve of the sample. The differential thermal analyzer used in this application is a Mettler-Toledo TGA / DSC3+ thermogravimetric and synchronous thermal analyzer, the standard used in the test is α-Al2O3 powder, the container for placing the sample is a platinum crucible, the ambient temperature of the instrument is 24°C, and the air humidity is ≤40%.

[0112] Stress test: In this application, the SLP 2000 (Luceo, Japan) stress meter is used to test the |CT_CV|, DOL_0, and |CT_AV| of chemically strengthened microcrystalline glass. The relevant parameter settings of the stress meter are: the wavelength of the light source is 518nm, the SOC (photoelastic coefficient) is set to 25.5, the refractive index is set according to the refractive index value of the sample to be tested, and the exposure time is 300μsec. Then, the tensile stress line density (CT_LD) value of the chemically strengthened microcrystalline glass is calculated by the calculation formula of the tensile stress line density mentioned above.

[0113] Deformation test: Tested by single strength test method, specifically, the chemically strengthened microcrystalline glass is placed on the bottom ring of the tensile testing machine (LT_850A), so that the round head of the pressure rod contacts the center of the main surface of the chemically strengthened microcrystalline glass, and the pressure rod movement speed is set to 50mm / min. Start the test software, click to start the test, and record the applied load and the corresponding deformation curve through the test software. Read the deformation of the chemically strengthened microcrystalline glass when the load is 10kgf. The deformation here refers to the displacement of the force point position on the main surface of the chemically strengthened microcrystalline glass in the force direction. The pressure rod used in this test method is a metal pressure rod with a diameter of 10mm, and the round head of the pressure rod is a hemisphere with a diameter of 10mm.

[0114] Test of the load borne when a certain amount of deformation occurs: The "load borne" here refers to the load that needs to be applied to the force point position in order for the main surface of the chemically strengthened microcrystalline glass to undergo a corresponding deformation along the force direction.

[0115] The test method of "load borne" is the same as the test method of deformation, and the test is carried out using the single strength test method. Specifically, the chemically strengthened microcrystalline glass is placed on the bottom ring of the tensile testing machine (LT_850A), so that the round head of the pressure rod contacts the center of the main surface of the chemically strengthened microcrystalline glass. The pressure rod movement speed is set to 50 mm / min, the test software is started, and the test is started. The test software records the curve of the applied load and the corresponding deformation. The load required to be applied when the deformation of the chemically strengthened microcrystalline glass sample is 0.40 mm is read, and recorded as the "load borne" (or the load offset during deformation) at the center of the main surface of the chemically strengthened microcrystalline glass when the deformation is 0.40 mm. The pressure rod used in this test method is a metal pressure rod with a diameter of 10 mm, and the round head of the pressure rod is a hemisphere with a diameter of 10 mm.

[0116] Without being bound by any theory, it is speculated that the process of glass deformation is actually the process of offsetting stress. When the cover glass is subjected to a certain force and deforms, the greater the offset stress, the smaller the force transmitted to the inner glass screen under the same impact, that is, the smaller the pressure on the inner glass screen, and the more conducive to avoiding the problem of failure of the inner glass screen. Similarly, when the cover glass is subjected to a certain force, the smaller the deformation, the less likely it is to squeeze the inner glass screen, and thus the less likely it is to cause the inner glass screen to fail.

[0117] In view of this, the present application provides a glass-ceramic having high mechanical strength, excellent optical properties and excellent deformation resistance and having lithium disilicate as the main crystal phase, a chemically strengthened glass-ceramic and its application. The glass-ceramic provided in the present application can obtain a chemically strengthened glass-ceramic with a high stress level after chemical strengthening.

[0118] As described above, in some embodiments of the present application, a glass-ceramic is provided, wherein the glass-ceramic contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the glass-ceramic; and the composition of the glass-ceramic, measured in molar percentage of oxides, includes:

[0119] SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol% , Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;

[0120] The composition of the microcrystalline glass satisfies the following condition: 2.00≤SiO2 / Li2O≤2.40, measured by the content of each oxide in the microcrystalline glass composition expressed as a molar percentage.

[0121] In the present application, by optimizing the glass formula, such as using a higher zirconium content and a lower aluminum content at a higher lithium content, and so on, while ensuring that the various components satisfy a specific content relationship and interact with each other, on the one hand, it is beneficial to ensure the precipitation of the desired content of lithium disilicate crystalline phase and limit the precipitation of other crystalline phases (such as petalite crystalline phase), thereby helping to ensure that microcrystalline glass with high intrinsic strength and excellent optical properties and with lithium disilicate as the main crystalline phase is obtained; on the other hand, it is beneficial to ensure that the microcrystalline glass satisfies a specific composition and structure, thereby ensuring that after chemical strengthening, chemically strengthened microcrystalline glass with a high stress level and excellent deformation resistance is prepared.

[0122] In some embodiments, the value of SiO2 / Li2O in the glass-ceramics can be, for example, 2.00, 2.01, 2.02, 2.05, 2.06, 2.07, 2.08, 2.09, 2.10, 2.11, 2.12, 2.13, 2.14, 2.15, 2.16, 2.17, 2.18, 2.19, 2.20, 2.25, 2.30 or 2.40, or can be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the desired performance of the present application can be obtained. Adopting a composition that satisfies this relationship is conducive to reducing the crystal size in the microcrystalline glass and improving the optical properties of the microcrystalline glass; at the same time, it is conducive to ensuring the precipitation of the main crystalline phase lithium disilicate crystals and can effectively reduce the precipitation of other crystalline phases (such as petalite crystals), which is conducive to ensuring that the microcrystalline glass obtains higher intrinsic strength and also helps the microcrystalline glass obtain a high stress level after chemical strengthening.

[0123] In the glass system of the present application, SiO2 is a glass network forming oxide and is an indispensable component of the glass network structure. At the same time, SiO2 is also indispensable as an important component of the lithium disilicate (Li2Si2O5) crystalline phase. Properly increasing the content of SiO2 can increase the structural stability and mechanical strength of the glass, while ensuring the precipitation of the desired content of lithium disilicate crystalline phase. However, excessive SiO2 will increase the viscosity of the substrate glass, making the glass melting more difficult, thereby reducing the formability of the substrate glass. Therefore, in order to ensure better forming and crystallization effects, the molar percentage of SiO2 is controlled at 55.00mol%-65.00mol%, preferably, the molar percentage of SiO2 is 60.00mol%-65.00mol%.

[0124] In some embodiments, the microcrystalline glass may contain 55.00mol%-65.00mol%, 58.00mol%-64.00mol%, 60.00mol%-65.00mol%, 61.00mol%-64.00mol%, 60.50mol%-64.00mol%, 61.50mol%-63.50mol%, 62.00mol%-64.00mol%, 63.00mol%-64.00mol% or 63.00mol%-65.00mol% SiO2. In some embodiments, the glass-ceramics may include 55.00 mol%, 56.00 mol%, 57.00 mol%, 58.00 mol%, 59.00 mol%, 60.00 mol%, 61.00 mol%, 62.00 mol%, 63.00 mol%, 64.00 mol%, 62.55 mol%, 62.58 mol%, 61.82 mol%, 61.72 mol%, 61.87 mol%, 61.76 mol%. %, 62.59mol%, 61.15mol%, 61.25mol%, 61.06mol%, 63.17mol%, 62.77mol%, 63.39mol%, 63.17mol%, 63.16mol%, 62.01mol% or 65.00mol% SiO2, or SiO2 within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.

[0125] In the glass system of the present application, Al2O3 is an optional component. The addition of an appropriate amount of Al2O3 helps stabilize the glass network structure and promotes the exchange of ions during chemical strengthening to a certain extent. However, excessive Al2O3 will increase the viscosity of the glass and easily lead to the precipitation of other crystalline phases, such as petalite, which will reduce the content of lithium disilicate crystalline phase and affect the interlocking structure of lithium disilicate. Therefore, the molar percentage of Al2O3 is controlled at 0.00mol%-2.00mol%.

[0126] In some embodiments, the microcrystalline glass may contain 0.00mol%-2.00mol%, 0.00mol%-1.60mol%, 0.00mol%-1.00mol%, 0.50mol%-1.60mol%, 0.50mol%-1.00mol%, 0.00mol%-0.50mol%, 1.20mol%-1.60mol%, 0.00mol%-1.30mol%, 0.00mol%-1.20mol% or 1.00mol%-2.00mol% Al2O3. In some embodiments, the microcrystalline glass may contain 0.00mol%, 0.50mol%, 0.70mol%, 0.85mol%, 0.95mol%, 1.00mol%, 1.10mol%, 1.20mol%, 1.30mol%, 1.40mol%, 1.50mol%, 1.60mol%, 1.80mol%, 1.55mol%, 1.38mol%, 1.41mol%, 1.37mol%, 1.39mol%, 1.43mol%, 1.23mol%, 1.42mol% or 2.00mol% Al2O3, or Al2O3 within the numerical range formed by any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0127] In the glass system of the present application, P2O5, as a nucleating agent, is an indispensable part. When its content is too little or too much, it will lead to poor crystallization effect and affect the optical properties of the obtained microcrystalline glass, such as reducing the transparency of the microcrystalline glass. Therefore, the molar percentage of P2O5 is controlled at 1.00mol%-3.00mol%, preferably 1.50mol%-2.50mol%.

[0128] In some embodiments, the glass-ceramics may include 1.00mol%-3.00mol%, 1.50mol%-3.00mol%, 1.60mol%-2.80mol%, 1.50mol%-2.50mol%, 1.60mol%-2.10mol%, 1.70mol%-2.20mol%, 1.50mol%-1.60mol%, 1.70mol%-3.00mol%, 1 .60mol%-2.50mol%, 1.70mol%-2.30mol%, 1.80mol%-2.00mol%, 2.00mol%-3.00mol%, 1.80mol%-1.90mol%, 1.60mol%-1.90mol%, 1.70mol%-1.90mol%, 1.75mol%-1.95mol% or 1.50mol%-2.00mol% P2O5. In some embodiments, the microcrystalline glass may contain 1.00 mol%, 1.20 mol%, 1.50 mol%, 1.70 mol%, 1.75 mol%, 1.80 mol%, 1.85 mol%, 1.95 mol%, 2.00 mol%, 2.10 mol%, 2.20 mol%, 2.30 mol%, 2.40 mol%, 2.50 mol%, 2.60 mol%, 2.80 mol%, 2.06 mol%, 1.87 mol%, 1.88 mol%, 1.86 mol%, 1.83 mol%, 1.89 mol%, 1.74 mol%, 1.51 mol% or 3.00 mol% of P2O5, or P2O5 within the numerical range formed by any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0129] In the glass system of the present application, ZrO2 is an intermediate oxide in glass formation, mainly as a nucleating agent and toughening agent, which plays a role in reducing the grain size and increasing the toughness of microcrystalline glass. However, when its content is too high, it will increase the difficulty of melting the substrate glass, such as causing a large amount of white precipitate to appear in the substrate glass, which is not conducive to obtaining microcrystalline glass with excellent optical properties. Therefore, the molar percentage of ZrO2 is controlled at 2.00mol%-6.00mol%, preferably 3.20mol%-6.00mol%.

[0130] In some embodiments, the microcrystalline glass may contain 2.00mol%-6.00mol%, 2.30mol%-5.80mol%, 2.50mol%-5.50mol%, 2.80mol%-5.30mol%, 2.90mol%-5.10mol%, 3.00mol%-5.50mol%, 3.10mol%-4.80mol%, 4.80mol%-6.00mol%, 4.00mol%-6.00mol%, 3.20mol%-5.30mol%, 3.50mol%-5.00mol%, 3.50mol%-5.80mol%, 4.00mol%-5.00mol% or 3.20mol%-6.00mol% ZrO2. In some embodiments, the glass-ceramics may include 2.00 mol%, 2.30 mol%, 2.50 mol%, 2.70 mol%, 2.90 mol%, 3.00 mol%, 3.10 mol%, 3.30 mol%, 3.50 mol%, 4.00 mol%, 4.50 mol%, 5.00 mol%, 5.50 mol%, 5.80 mol%, 2.58 mol%, 4.68 mol%, 4.66 mol%, 4.61 mol%, 3.16 mol%, 3.72 mol%,

[0131] 4.21mol%, 4.57mol%, 5.10mol%, 5.54mol%, 4.72mol%, 2.18mol%, 2.36mol%, 3.31mol%, 4.63mol% or 6.00mol% ZrO2, or ZrO2 within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained.

[0132] In the glass system of the present application, CaO is an optional component of the network exo-oxide formed by the glass. An appropriate amount of CaO helps to reduce the high temperature viscosity of the glass, increase the density of the glass, and is beneficial to the glass molding. At the same time, it can enhance the network structure and enhance the stress benefit of the chemical strengthening process. However, excessive CaO will cause the crystallinity of the glass to drop sharply and the intrinsic strength will be affected. Therefore, the molar percentage of CaO is controlled at 0.00mol%-5.00mol%.

[0133] In some embodiments, the glass-ceramics may contain 0.00mol%-5.00mol%, 0.10mol%-4.00mol%, 0.00mol%-2.50mol%, 0.50mol%-3.80mol%, 0.00mol%-4.00mol%, 0.80mol%-2.00mol%, 0.00mol%-1.60mol%, 0.00mol%-1.00mol%, 1.50mol%-4.00mol%, 0.00mol%-2.00mol%, 1.00mol%-4.00mol% or 0.10mol%-5.00mol% CaO. In some embodiments, the microcrystalline glass may contain 0.00mol%, 0.10mol%, 0.50mol%, 0.70mol%, 0.85mol%, 0.95mol%, 1.00mol%, 1.10mol%, 1.20mol%, 1.30mol%, 1.40mol%, 1.50mol%, 1.60mol%, 1.80mol%, 2.00mol%, 2.50mol%, 3.00mol%, 4.00mol%, 3.72mol%, 0.94mol%, 0.92mol%, 0.93mol%, 1.83mol%, 2.67mol% or 5.00mol% CaO, or CaO within the numerical range formed by any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0134] In the glass system of the present application, Li2O is an essential component and a network exo-oxide formed by glass. It can not only provide free oxygen, improve the viscosity of the glass, and promote the melting and clarification of the glass liquid, but also is one of the main components for the formation of lithium disilicate crystals. At the same time, Li2O can also provide alkali metal lithium ions for ion exchange with large-radius ions in the molten salt bath, which is an important factor affecting the stress level that can be obtained by chemically strengthened microcrystalline glass. However, excessive Li2O may cause the stability of the glass crystallization process to deteriorate, and even precipitate other undesirable crystalline phases, which deteriorates the optical properties of the microcrystalline glass. Therefore, the molar percentage of Li2O is controlled at 27.00mol%-32.00mol%, preferably 28.00mol%-31.00mol%.

[0135] In some embodiments, the glass-ceramics may include 27.00 mol%-32.00 mol%, 27.50 mol%-31.00 mol%, 27.00 mol%-30.00 mol%, 27.50 mol%-29.50 mol%, 28.00 mol%-31.00 mol%, 28.50 mol%-31.00 mol%, 29.00 mol%-30.50 mol% or 29.50 mol%-32.00 mol% Li2O. In some embodiments, the glass-ceramics may contain 27.00 mol%, 27.50 mol%, 28.00 mol%, 28.50 mol%, 29.00 mol%, 29.50 mol%, 30.00 mol%, 30.50 mol%, 31.00 mol%, 31.50 mol%, 27.54 mol%, 28.59 mol%, 29.52 mol%, 29.08 mol%, 29.80 mol%, 29.93 mol%, 29.30 mol%, 31.51 mol%, 30.22 mol%, 29.66 mol%, 29.25 mol% or 32.00 mol% of Li2O, or Li2O within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0136] In the glass system of the present application, MgO is an optional component. An appropriate amount of MgO can adjust the glass phase composition in the microcrystalline glass. However, excessive MgO will affect the growth of crystals and the crystalline structure of the microcrystalline glass. Therefore, the molar percentage of MgO is controlled at 0.00 mol%-2.00 mol%.

[0137] In some embodiments, the glass-ceramics may contain 0.00mol%-2.00mol%, 0.00mol%-1.60mol%, 0.50mol%-1.60mol%, 0.80mol%-1.50mol%, 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.10mol%-1.10mol%, 0.10mol%-1.50mol% or 0.00mol%-1.40mol% of MgO. In some embodiments, the glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.34 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol% or 2.00 mol% of MgO, or MgO within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0138] In the glass system of the present application, ZnO is one of the optional components as a network intermediate. An appropriate amount of ZnO can combine with free oxygen to adjust the glass structure, and can remain in the glass phase of the microcrystalline glass to increase the glass viscosity. However, excessive ZnO will affect the growth of crystals and the crystal phase structure of the microcrystalline glass. Therefore, the molar percentage of ZnO is controlled to be between 0.00mol% and 2.00mol%.

[0139] In some embodiments, the glass-ceramics may contain 0.00mol%-2.00mol%, 0.00mol%-1.70mol%, 0.50mol%-1.60mol%, 0.80mol%-1.50mol%, 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.10mol%-1.10mol%, 0.10mol%-1.50mol% or 0.00mol%-1.40mol% ZnO. In some embodiments, the glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.67 mol%, 1.80 mol% or 2.00 mol% of ZnO, or ZnO within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0140] In the glass system of the present application, Na2O is an optional component and a network exo-oxide. An appropriate amount of Na2O can provide free oxygen, improve the viscosity of the glass, promote the melting and clarification of the glass liquid, and also adjust the chemical strengthening rate. However, excessive Na2O will not only reduce the crystallinity of the microcrystalline glass, but also affect the chemical strengthening effect. Therefore, the molar percentage of Na2O is controlled to be between 0.00mol% and 3.00mol%.

[0141] In some embodiments, the glass-ceramics may contain 0.00mol%-3.00mol%, 0.00mol%-2.80mol%, 0.00mol%-1.00mol%, 0.10mol%-2.70mol%, 0.50mol%-1.60mol%, 0.60mol%-1.00mol%, 2.50mol%-3.00mol% or 0.00mol%-0.50mol% of Na2O. In some embodiments, the glass-ceramics may contain 0.00 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol%, 2.00 mol%, 2.50 mol%, 2.60 mol% or 3.00 mol% of Na2O, or Na2O within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0142] In the glass system of the present application, K2O is an oxide outside the glass network and is one of the optional components. An appropriate amount of K2O can provide free oxygen to increase the oxygen-silicon ratio in the glass structure, but too much K2O will affect the network structure of the glass, and affect the optical properties, thermal stability, chemical stability, mechanical strength and weather resistance of the glass. Therefore, the molar percentage of K2O is controlled to be between 0.00 mol% and 1.00 mol%.

[0143] In some embodiments, the glass-ceramics may contain 0.00mol%-1.00mol%, 0.50mol%-1.00mol%, 0.00mol%-0.50mol%, 0.85mol%-1.00mol% or 0.00mol%-0.15mol% K2O. In some embodiments, the glass-ceramics may contain 0.00mol%, 0.15mol%, 0.50mol%, 0.70mol%, 0.85mol%, 0.92mol%, 0.95mol% or 1.00mol% K2O, or K2O within the numerical range formed by any two of the above specific numerical values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0144] In the glass system of the present application, B2O3 is an optional component. An appropriate amount of B2O3 can be used as a flux and / or softener to help improve the molding and hot bending effects of the glass. However, excessive B2O3 will cause uncontrollable crystallization process and deteriorate the optical properties of the microcrystalline glass. Therefore, the molar percentage of B2O3 is controlled at 0.00mol%-1.00mol%.

[0145] In some embodiments, the glass-ceramics may contain 0.00mol%-1.00mol%, 0.00mol%-0.50mol%, 0.50mol%-1.00mol%, 0.10mol%-0.85mol%, 0.85mol%-1.00mol% or 0.25mol%-0.75mol% B2O3. In some embodiments, the glass-ceramics may contain 0.00mol%, 0.10mol%, 0.25mol%, 0.50mol%, 0.60mol%, 0.65mol%, 0.70mol%, 0.75mol%, 0.85mol%, 0.95mol% or 1.00mol% B2O3, or B2O3 within the numerical range formed by any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0146] In the glass system of the present application, SrO is an alkaline earth metal oxide as an optional component. An appropriate amount of SrO can play a role in regulating the glass phase composition in the microcrystalline glass, which helps to increase the density of the microcrystalline glass and increase its Young's modulus. At the same time, it is also beneficial to reduce the expansion softening point of the microcrystalline glass, and then facilitate the hot bending of the microcrystalline glass into 3D curved microcrystalline glass. However, excessive SrO will deteriorate the optical properties of the microcrystalline glass, so the molar percentage of SrO is controlled at 0.00mol%-2.00mol%.

[0147] In some embodiments, the glass-ceramics may contain 0.00mol%-2.00mol%, 0.10mol%-2.00mol%, 0.00mol%-1.00mol%, 0.10mol%-1.00mol%, 0.30mol%-1.90mol%, 0.40mol%-1.20mol%, 1.20mol%-2.00mol%, 0.00mol%-0.30mol%, 0.85mol%-1.40mol%, 0.85mol%-1.90mol%, 0.50mol%-1.20mol% or 1.00mol%-2.00mol% SrO. In some embodiments, the glass-ceramics may contain 0.00 mol%, 0.30 mol%, 0.46 mol%, 0.50 mol%, 0.70 mol%, 0.85 mol%, 0.92 mol%, 0.95 mol%, 1.00 mol%, 1.10 mol%, 1.20 mol%, 1.30 mol%, 1.40 mol%, 1.50 mol%, 1.60 mol%, 1.80 mol%, 1.83 mol% or 2.00 mol% of SrO, or SrO within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0148] In some embodiments, the composition of the microcrystalline glass includes, in terms of molar percentage of oxides: SiO2: 60.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-4.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%. By making the microcrystalline glass meet the above-mentioned composition, not only can the microcrystalline glass be given high intrinsic strength and excellent optical properties, but also its chemical strengthening effect can be guaranteed, ensuring that the microcrystalline glass obtains a higher stress level after chemical strengthening, thereby obtaining higher mechanical strength properties and excellent deformation resistance.

[0149] In some embodiments, the composition of the glass-ceramics described in the present application may further include other components on the basis of the above composition range. For example, in some specific embodiments, the composition of the glass-ceramics further includes, in terms of molar percentage of oxides: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

[0150] In the glass system of the present application, the selective addition of an appropriate amount of Y2O3, La2O3 or Ta2O5 helps to increase the density of the microcrystalline glass and increase its Young's modulus, but it may also increase the refractive index of the microcrystalline glass and reduce the optical properties of the microcrystalline glass. Therefore, the molar percentage of Y2O3, La2O3 or Ta2O5 is controlled at 0.00mol%-1.00mol%.

[0151] In some embodiments, in the glass-ceramics, the molar percentage of Y2O3, La2O3 or Ta2O5 can be 0.00mol%, 0.10mol%, 0.20mol%, 0.30mol%, 0.40mol%, 0.46mol%, 0.50mol%, 0.53mol%, 0.60mol%, 0.70mol%, 0.75mol%, 0.80mol%, 0.85mol%, 0.90mol%, 0.95mol% or 1.00mol%, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0152] In some embodiments, the composition of the glass-ceramics includes, in terms of molar percentage of oxides: SiO2: 60.50mol%-64.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-2.50mol%, ZrO2: 3.20mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-1.00mol%. mol%, K2O: 0.00mol%-1.00mol%, Li2O: 28.00mol%-31.00mol%, CaO: 0.00mol%-2.50mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%, Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%. By making the microcrystalline glass meet the above composition, it is more conducive to preparing chemically strengthened microcrystalline glass with higher stress level, and further conducive to ensuring that the prepared chemically strengthened microcrystalline glass has excellent mechanical strength and deformation resistance.

[0153] In some embodiments of the present application, the composition of the glass-ceramics also satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the glass-ceramics composition: 0.90≤SiO2+Li2O≤0.96. The use of a composition that satisfies this relationship is conducive to ensuring that the desired content of lithium disilicate crystals is precipitated in the glass-ceramics, and can effectively reduce the precipitation of other crystals (such as petalite crystals), which is conducive to ensuring that the glass-ceramics obtains higher intrinsic strength and optical properties, and is also conducive to obtaining a high stress level for the glass-ceramics after chemical strengthening. At the same time, it is also conducive to ensuring that the substrate glass does not lose transparency when the glass-ceramics is prepared by heat treatment, or that the substrate glass does not lose transparency during the melting process. In some embodiments, the value of SiO2+Li2O may be, for example, 0.900, 0.904, 0.905, 0.910, 0.915, 0.920, 0.925, 0.930, 0.935, 0.940, 0.945, 0.950, or 0.960, or may be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0154] In some embodiments of the present application, the composition of the glass-ceramics is also satisfied by the content expressed by the molar percentage of each oxide in the composition of the glass-ceramics: Al2O3 / SiO2≤0.030. By adjusting the content relationship of Al2O3 and SiO2, while stabilizing the glass network structure, it is beneficial to ensure the formation of the desired crystalline phase structure, and it is also beneficial to make the glass-ceramics obtain a high stress level after chemical strengthening, thereby ensuring that the glass-ceramics obtains high mechanical strength performance and excellent deformation resistance. In some embodiments, the value of Al2O3 / SiO2 can be, for example, 0, 0.005, 0.010, 0.015, 0.020, 0.025 or 0.030, or it can be a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the performance required by the present application can be obtained.

[0155] In some embodiments of the present application, the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, also satisfies: 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50, preferably, 0.32≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.20, and more preferably, 0.36≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.10. By adjusting the specific content relationship between CaO, ZrO2, and Al2O3, which have a strengthening or toughening effect on the glass structure, it is beneficial to better play the role of each component, thereby ensuring the high intrinsic strength of the glass-ceramics and the high stress level after strengthening, and further ensuring that the glass-ceramics obtains high mechanical strength properties and excellent deformation resistance. In some embodiments, the value of ZrO2 / (CaO+ZrO2+Al2O3) can be, for example, 0.31, 0.32, 0.34, 0.36, 0.37, 0.33, 0.83, 0.77, 0.67, 0.69, 0.62, 0.75, 0.59, 0.79, 0.80, 1.00, 0.35, 0.66, 0.50, 0.70, 0.40, 0.60, 0.90, 1.10, 1.20, 1.30, 1.40 or 1.50, or can be a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained.

[0156] In some embodiments of the present application, the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, also satisfies: 0.10≤ZrO2 / (100%-3×Li2O)≤0.60, preferably, 0.12≤ZrO2 / (100%-3×Li2O)≤0.52, and more preferably, 0.16≤ZrO2 / (100%-3×Li2O)≤0.50. By adjusting ZrO2 and Li2O to meet a specific content relationship, it is beneficial to better exert the nucleation and / or toughening effect of ZrO2 while ensuring that the glass-ceramics forms a desired crystalline phase structure and achieves excellent optical properties, thereby ensuring that the glass-ceramics has high intrinsic strength, and thus ensuring that the glass-ceramics obtains high mechanical strength and excellent deformation resistance. In some embodiments, the value of ZrO2 / (100%-3×Li2O) can be, for example, 0.10, 0.12, 0.15, 0.33, 0.44, 0.40, 0.25, 0.35, 0.41, 0.37, 0.46, 0.48, 0.39, 0.13, 0.43, 0.42, 0.50, 0.52, 0.56 or 0.60, or can be a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained.

[0157] In some embodiments of the present application, the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, also satisfies: 0.034≤ZrO2 / SiO2≤0.100, preferably, 0.035≤ZrO2 / SiO2≤0.095, and more preferably, 0.055≤ZrO2 / SiO2≤0.095. By adjusting ZrO2 and SiO2 to meet a specific content relationship, it is beneficial to better exert the toughening effect of ZrO2 while ensuring that the glass-ceramics forms a desired crystalline phase structure and achieves excellent optical properties, thereby ensuring that the glass-ceramics has high intrinsic strength, and further ensuring that the glass-ceramics obtains high mechanical strength and excellent deformation resistance. In some embodiments, the value of ZrO2 / SiO2 may be, for example, 0.041, 0.075, 0.051, 0.060, 0.067, 0.083, 0.091, 0.035, 0.037, 0.052, 0.034, 0.100, 0.095 or 0.055, or may be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained.

[0158] In some embodiments of the present application, the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, also satisfies the following conditions: CaO+Al2O3≤0.065, preferably, CaO+Al2O3≤0.055, and more preferably, CaO+Al2O3≤0.050. By controlling the total content of CaO and Al2O3 to meet specific requirements, it is beneficial to avoid affecting the crystallization of the glass-ceramics while exerting their reinforcing effects, thereby ensuring that the glass-ceramics achieves the desired crystalline phase structure, and further helps to ensure that the glass-ceramics obtains high mechanical strength and excellent deformation resistance. In some embodiments, the value of CaO+Al2O3 may be, for example, 0.000, 0.053, 0.009, 0.014, 0.023, 0.032, 0.041, 0.012, 0.024, 0.050, 0.055, or 0.065, or may be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0159] In some embodiments of the present application, the composition of the glass-ceramics also satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics: (CaO+Al2O3) / Li2O≤0.25, preferably, (CaO+Al2O3) / Li2O≤0.20, and more preferably, (CaO+Al2O3) / Li2O≤0.14. By adjusting CaO, Al2O3, and Li2O to meet a specific content relationship, it is beneficial to ensure that the desired content of lithium disilicate crystal phase is precipitated in the glass-ceramics while exerting the strengthening effect of CaO and / or Al2O3, thereby ensuring that the glass-ceramics achieves the desired crystal phase structure, and further helps to ensure that the glass-ceramics obtains high mechanical strength performance and excellent deformation resistance. In some embodiments, the value of (CaO+Al2O3) / Li2O may be, for example, 0.00, 0.19, 0.03, 0.05, 0.08, 0.11, 0.15, 0.04, 0.14, 0.16, 0.20, or 0.25, or may be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass having the desired performance of the present application can be obtained.

[0160] In some embodiments of the present application, the composition of the glass-ceramics, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics, also satisfies: 0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40, preferably, 0.14≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.16, and more preferably, 0.50≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤3.00. By adjusting ZrO2, Na2O, SiO2, and Li2O to meet a specific content relationship, it is beneficial to better play the role of each component, to enable the glass-ceramics to obtain high intrinsic strength and excellent optical properties, and to enable the glass-ceramics to obtain a high stress level and excellent deformation resistance after chemical strengthening. In some embodiments, the value of (ZrO2-Na2O) / (SiO2-2×Li2O) can be, for example, 0.12, 0.35, 0.87, 2.08, 1.72, 0.15, 1.55, 2.63, 2.73, 1.03, 0.28, 6.15, 0.86, 1.21, 6.20, 6.38, 0.14, 6.16, 0.50, 6.40 or 3.00, or can be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained.

[0161] In some embodiments of the present application, the composition of the glass-ceramics also satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the composition of the glass-ceramics: Na2O / SiO2≤0.05, preferably, Na2O / SiO2≤0.04, and more preferably, Na2O / SiO2≤0.02. By adjusting Na2O and SiO2 to meet a specific content relationship, it is more conducive to the glass-ceramics to obtain a high stress level and excellent deformation resistance after chemical strengthening. In some embodiments, the value of Na2O / SiO2 may be, for example, 0.00, 0.01, 0.02, 0.03, 0.04 or 0.05, or may be a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges may be combined with any other ranges, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained.

[0162] In some embodiments of the present application, the density of the microcrystalline glass is ρ≥2.50 g / cm 3 Preferably, the density ρ of the microcrystalline glass is 2.50 g / cm3 ~2.75g / cm 3 In some embodiments of the present application, the refractive index of the microcrystalline glass is ≤1.60. Microcrystalline glass satisfying this density and / or refractive index can ensure high intrinsic strength and excellent optical properties.

[0163] In some embodiments, the density ρ of the microcrystalline glass can be 2.50 g / cm 3 , 2.54g / cm 3 , 2.55g / cm 3 , 2.56g / cm 3 , 2.57g / cm 3 , 2.58g / cm 3 , 2.59g / cm 3 , 2.60g / cm 3 , 2.61g / cm 3 , 2.62g / cm 3 , 2.63g / cm 3 , 2.64g / cm 3 , 2.65g / cm 3 , 2.70g / cm 3 or 2.75g / cm 3 , or a value above any of the above specific values, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass with the required performance of the present application can be obtained.

[0164] In some embodiments, the refractive index of the glass-ceramics may be 1.50, 1.51, 1.52, 1.53, 1.54, 1.55, 1.56, 1.57, 1.58, 1.59 or 1.60, or a value below any of the above specific values, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics with the required performance of the present application can be obtained.

[0165] In some embodiments of the present application, the crystallinity of the glass-ceramics is 30.00wt%-90.00wt%, preferably, the crystallinity is 50.00wt%-90.00wt%, and more preferably, the crystallinity is 65.00wt%-90.00wt%. A higher content of crystalline phase is beneficial to improving the mechanical strength performance of the glass-ceramics while ensuring the excellent optical properties of the glass-ceramics. In some embodiments, the crystallinity of the glass-ceramics can be 30.00wt%-90.00wt%, 45.00wt%-85.00wt%, 50.00wt%-90.00wt%, 55.00wt%-85.00wt%, 60.00wt%-85.00wt%, 65.00wt%-90.00wt%, 70.00wt%-90.00wt% or 68.00wt%-85.00wt%. In some embodiments, the crystallinity of the glass-ceramics can be 30.00wt%, 35.00wt%, 40.00wt%, 45.00wt%, 50.00wt%, 55.00wt%, 60.00wt%, 65.00wt%, 70.00wt%, 75.00wt%, 80.00wt%, 85.00wt% or 90.00wt%, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics with the required performance of the present application can be obtained.

[0166] In some embodiments of the present application, "the main crystalline phase is lithium disilicate" or "the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the microcrystalline glass" and similar expressions mean that the lithium disilicate crystalline phase accounts for more than about 70 weight percent (wt %) of all crystalline phases of the microcrystalline glass according to the embodiments of the present application.

[0167] In some embodiments of the present application, non-limiting examples of other possible crystalline phases in the microcrystalline glass include: petalite crystalline phase, and / or, lithium phosphate crystalline phase. In some embodiments, the microcrystalline glass also contains a petalite crystalline phase, preferably the weight percentage of the petalite crystalline phase in the microcrystalline glass is less than or equal to 20%, and more preferably, the weight percentage of the petalite crystalline phase in the microcrystalline glass can be less than or equal to 15%, less than or equal to 10%, or less than or equal to 5%. By controlling the precipitation of other crystalline phases, it is more conducive to ensuring that lithium disilicate forms a desired interlocking structure, thereby ensuring that the microcrystalline glass obtains high mechanical strength performance, excellent optical properties and excellent deformation resistance.

[0168] In some embodiments of the present application, in the glass-ceramics, the average crystal size is ≤100nm, preferably, the average crystal size is ≤50nm, and more preferably, the average crystal size is 15nm to 45nm. Meeting a smaller average crystal size is conducive to ensuring that the glass-ceramics has excellent optical properties. In some embodiments, the average crystal size can be 10nm to 100nm, 20nm to 90nm, 30nm to 80nm, 40nm to 60nm, 10nm to 30nm, 10nm to 20nm, 5nm to 35nm, 15nm to 35nm or 15nm to 45nm. In some embodiments, the average crystal size can be 5nm, 10nm, 15nm, 20nm, 25nm, 30nm, 35nm, 40nm, 45nm, 50nm, 55nm, 60nm, 70nm, 80nm, 90nm or 100nm, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the desired performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass with the desired performance of the present application can be obtained.

[0169] In some embodiments of the present application, the Young's modulus of the glass-ceramics is ≥100.00GPa, preferably the Young's modulus of the glass-ceramics is ≥110.00GPa, preferably the Young's modulus of the glass-ceramics is ≥110.00GPa, more preferably, the Young's modulus of the glass-ceramics is 114GPa-130GPa. Having a higher Young's modulus indicates that the glass-ceramics has a higher intrinsic strength, which is conducive to obtaining higher mechanical strength properties and excellent deformation resistance. In some embodiments, the Young's modulus of the glass-ceramics can be 100.00GPa-150GPa, 105.00GPa-140GPa, 110.00GPa-130GPa, 114GPa-130GPa or 114.00GPa-125GPa. In some embodiments, the Young's modulus of the glass-ceramics may be 100.00 GPa, 105.00 GPa, 110.00 GPa, 114.00 GPa, 115.00 GPa, 120.00 GPa, 125.00 GPa, 130.00 GPa, 140.00 GPa or 150.00 GPa, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the glass-ceramics or chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that, in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the glass-ceramics with the required performance of the present application can be obtained.

[0170] In some embodiments of the present application, at a thickness of 0.5 mm, the b value of the microcrystalline glass is ≤1.0, preferably ≤0.8. The microcrystalline glass that meets the optical b value can ensure better optical performance and display effects, and is suitable for use in display screens that require display effects. In some embodiments, at a thickness of 0.5 mm, the b value of the microcrystalline glass can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1.0, or a value below any of the above specific values, or a value within the numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass with the required performance of the present application can be obtained.

[0171] In some embodiments of the present application, the microcrystalline glass is transparent in the visible light range; at a thickness of 0.5 mm, for light with a wavelength of 550 nm, the transmittance of the microcrystalline glass is ≥ 85.00%, preferably, the transmittance of the microcrystalline glass is ≥ 90.00%. Microcrystalline glass that meets this transmittance can ensure good light transmittance and transparency, and is suitable for use in display screens that require display effects. The "visible light range" here refers to light in the 360nm-740nm band.

[0172] In some embodiments, at a thickness of 0.5 mm, for light of a wavelength of 550 nm, the transmittance of the microcrystalline glass can be 85.00%, 86.00%, 87.00%, 88.00%, 89.00%, 90.00%, 90.50%, 91.00% or 92.00%, or a value within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the microcrystalline glass or chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass with the required performance of the present application can be obtained.

[0173] The microcrystalline glass of the present application has a high transmittance and a low b value, both of which indicate that the microcrystalline glass of the present application has excellent optical properties and good uniformity, is in a transparent state, and can meet the application requirements of display cover glass.

[0174] In some embodiments of the present application, the upper limit crystallization temperature of the substrate glass corresponding to the microcrystalline glass is between 1000° C. and 1100° C. Meeting this upper limit crystallization temperature range is conducive to industrial mass production.

[0175] In some embodiments of the present application, the expansion softening point of the microcrystalline glass is between 750°C and 850°C. Preferably, the expansion softening point of the microcrystalline glass is between 750°C and 830°C. A suitable expansion softening point is conducive to 3D hot bending of the microcrystalline glass to obtain 3D curved microcrystalline glass with high strength performance. In some embodiments, the expansion softening point of the microcrystalline glass can be 750°C, 760°C, 770°C, 780°C, 790°C, 800°C, 810°C, 820°C, 830°C, 840°C or 850°C, or a value within the numerical range formed by any two of the above specific values ​​as endpoints. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the microcrystalline glass with the required performance of the present application can be obtained.

[0176] In the present application, the microcrystalline glass can be prepared into a 3D curved microcrystalline glass after being subjected to a heat bending treatment. When the product composition is measured in terms of the molar percentage of oxides, the composition of the 3D curved microcrystalline glass is the same or substantially the same as that of the microcrystalline glass.

[0177] The glass-ceramics of the present application can be prepared by heat treating a substrate glass. The composition of the substrate glass used is the same or substantially the same as that of the glass-ceramics in terms of the molar percentage of oxides.

[0178] In the present application, the substrate glass can be prepared by the molding method in the prior art, and the present application has no restrictions on this. For example, the molding method may include but is not limited to: float, overflow, rolling or pouring, etc. Exemplarily, the raw materials and the clarifier can be mixed evenly (the uniformity is above 98%), melted, and annealed after molding to obtain the substrate glass. Further, the process parameters may include: the melting temperature is 1480℃-1680℃, the annealing temperature is 450℃-650℃, and the annealing temperature is kept at 10h-48h. Further, the clarifier may include but is not limited to one or more of sodium chloride, tin oxide, antimony oxide or arsenic oxide, and the amount of the clarifier added may be 0-1wt% of the total amount of the raw materials.

[0179] In the present application, when the substrate glass is heat-treated to prepare microcrystalline glass, the heat treatment can be carried out in a crystallization furnace or an annealing furnace, for example, and the heat treatment method can include but is not limited to one-step heat treatment, two-step heat treatment or multi-step heat treatment, for example, it can include two-step heat treatment of nucleation treatment and then crystallization treatment. The process conditions of the heat treatment can include but are not limited to: the nucleation temperature can be 500℃-700℃, the nucleation holding time can be 10min~1440min; the crystallization temperature can be 600℃-800℃, and the crystallization holding time can be 5min~1440min; the heating rate of the whole process can be 5℃ / min-20℃ / min, and the cooling rate can be 0.1℃ / min-3℃ / min. After the heat treatment, those skilled in the art can also perform other conventional steps to obtain microcrystalline glass samples that meet the required specifications or requirements, such as cutting, CNC processing (computer numerical control, i.e., CNC machine tools) or polishing.

[0180] In the present application, a chemically strengthened microcrystalline glass is also provided, wherein the composition at the center of the chemically strengthened microcrystalline glass is the same as the composition of the microcrystalline glass described above, the chemically strengthened microcrystalline glass includes a compressive stress layer region extending from the surface of the chemically strengthened microcrystalline glass to the compression depth, and has tensile stress inside the chemically strengthened microcrystalline glass.

[0181] It should be understood that the composition of the surface of the glass-ceramic article after chemical strengthening may be different from the composition of the glass-ceramic before it undergoes the ion exchange process. This is because, during the ion exchange process, one type of alkali metal ion (e.g., Li + Or Na + ) are replaced by larger alkali metal ions (e.g., Na + or K + ) is replaced. However, in an embodiment, the glass composition and phase assembly at the depth center or near the depth center of the microcrystalline glass product will still have the composition and phase assembly of the newly formed microcrystalline glass. That is to say, in the present application, the composition (e.g., the composition of the tensile stress layer) and phase assembly at the center of the chemically strengthened microcrystalline glass that has been chemically strengthened are the same or substantially the same as those of the newly formed microcrystalline glass.

[0182] In the present application, the chemically strengthened glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; in terms of molar percentage of oxides, the composition at the center of the chemically strengthened glass-ceramics includes: SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol% ol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol% , Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%;

[0183] The composition at the center of the chemically strengthened glass-ceramics, expressed in terms of the content as a molar percentage of oxides, satisfies: 2.00≤SiO2 / Li2O≤2.40, preferably, 2.00≤SiO2 / Li2O≤2.30, and more preferably, 2.02≤SiO2 / Li2O≤2.20.

[0184] In some embodiments of the present application, the composition at the center of the chemically strengthened glass-ceramics, expressed in terms of the content expressed in molar percentage of the oxide, further satisfies: 0.90≤SiO2+Li2O≤0.96; and / or, Al2O3 / SiO2≤0.030; and / or, 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50; and / or, 0.10≤ZrO2 / (100 %-3×Li2O)≤0.60;and / or,0.034≤ZrO2 / SiO2≤0.100;and / or,CaO+Al2O3≤0.065;and / or,(CaO+Al2O3) / Li2O≤0.25;and / or,0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40;and / or,Na2O / SiO2≤0.05。

[0185] In some embodiments of the present application, the composition at the center of the chemically strengthened glass-ceramics includes, in terms of molar percentage of oxides: SiO2: 60.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-4.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%.

[0186] In some embodiments of the present application, the composition at the center of the chemically strengthened glass-ceramics further includes, in terms of molar percentage of oxides: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

[0187] In some embodiments of the present application, the composition at the center of the chemically strengthened microcrystalline glass includes, in terms of molar percentage of oxides: SiO2: 60.50mol%-64.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.50mol%-2.50mol%, ZrO2: 3.20mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol %-1.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 28.00mol%-31.00mol%, CaO: 0.00mol%-2.50mol%, B2O3: 0.00mol%-1.00 mol%, SrO: 0.00mol%-2.00mol%, Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

[0188] In some embodiments of the present application, the chemically strengthened glass-ceramics has a DOL_0 of 0.18t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramics. In some embodiments, the depth of the compressive stress layer DOL_0 of the chemically strengthened glass-ceramics may be 0.18t-0.25t, 0.20t-0.25t, 0.21t-0.24t, 0.21t-0.25t or 0.22t-0.25t. Exemplarily, when the thickness of the chemically strengthened glass-ceramics is 0.5 mm, the DOL_0 of the chemically strengthened glass-ceramics may be 0.100 mm, 0.105 mm, 0.110 mm, 0.112 mm, 0.113 mm, 0.114 mm, 0.115 mm, 0.116 mm, 0.117 mm, 0.118 mm, 0.119 mm, 0.120 mm, 0.121 mm, 0.122 mm, 0.123 mm, 0.124 mm or 0.125 mm, or a value within the numerical range formed by any two of the above specific values ​​as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The DOL_0 of the chemically strengthened glass-ceramics is within the above range, which indicates that the chemically strengthened glass-ceramics has a high depth of compressive stress layer, which is more conducive to offsetting the energy driving crack propagation, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0189] In some embodiments of the present application, the chemically strengthened glass-ceramics has a |CT_AV| of 85MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress; preferably, it has a |CT_AV| of 90MPa-200MPa. In some embodiments, the chemically strengthened glass-ceramics has a |CT_AV| of 85MPa-200MPa, 90MPa-200MPa, 90MPa-180MPa, 100MPa-150MPa, 130MPa-180MPa, 85MPa-100MPa, 85MPa-120MPa, 90MPa-150MPa, 95MPa-180MPa, 100MPa-140MPa, 130MPa-200MPa, or 120MPa-140MPa. In some embodiments, the chemically strengthened glass-ceramics has a |CT_AV| of 85MPa, 90MPa, 100MPa, 110MPa, 120MPa, 130MPa, 140MPa, 150MPa, 160MPa, 170MPa, 180MPa, 190MPa or 200MPa, or a |CT_AV| within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the required performance of the present application can be obtained. The |CT_AV| of the chemically strengthened glass-ceramics is within the above range, indicating that the chemically strengthened glass-ceramics has a higher tensile stress level, reflecting that it has a higher surface stress level, and the higher surface compressive stress level can offset the more residual energy of falling, extrusion, impact or collision, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0190] In some embodiments of the present application, the chemically strengthened glass-ceramics has a CT_LD of 50000 MPa / mm-100000 MPa / mm, where CT_LD is a tensile stress linear density; preferably, it has a CT_LD of 55000 MPa / mm-100000 MPa / mm. In some embodiments, the chemically strengthened glass-ceramics has a CT_LD of 50000MPa / mm-100000MPa / mm, 55000MPa / mm-95000MPa / mm, 60000MPa / mm-90000MPa / mm, 65000MPa / mm-85000MPa / mm, 70000MPa / mm-80000MPa / mm, 65000MPa / mm-100000MPa / mm, 60000MPa / mm-80000MPa / mm or 60000MPa / mm-100000MPa / mm. In some embodiments, the chemically strengthened glass-ceramics has a CT_LD of 50000MPa / mm, 55000MPa / mm, 60000MPa / mm, 65000MPa / mm, 70000MPa / mm, 75000MPa / mm, 80000MPa / mm, 85000MPa / mm, 90000MPa / mm, 95000MPa / mm or 100000MPa / mm, or a CT_LD within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. The range of CT_LD of the chemically strengthened glass-ceramics is within the above range, indicating that the tensile stress stored inside the chemically strengthened glass-ceramics is relatively dense, indicating that the chemically strengthened glass-ceramics has a higher surface stress level, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0191] In some embodiments of the present application, the chemically strengthened glass-ceramics has a |CT_CV| of 120MPa-320MPa, preferably, the chemically strengthened glass-ceramics has a |CT_CV| of 135MPa-300MPa, and more preferably, the chemically strengthened glass-ceramics has a |CT_CV| of 160MPa-300MPa. |CT_CV| refers to the absolute value of the maximum tensile stress. In some embodiments, the chemically strengthened glass-ceramics has a |CT_CV| of 120MPa-320MP, 135MPa-300MPa, 160MPa-300MPa, 170MPa-285MPa, 180MPa-270MPa, 120MPa-250MPa or 165MPa-290MPa. In some embodiments, the chemically strengthened glass-ceramics has a |CT_CV| of 120MPa, 135MPa, 150MPa, 160MPa, 170MPa, 180MPa, 190MPa, 200MPa, 210MPa, 220MPa, 230MPa, 240MPa, 250MPa, 260MPa, 270MPa, 280MPa, 290MPa or 300MPa, or a |CT_CV| within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened glass-ceramics with the performance required by the present application can be obtained. The range of |CT_CV| of the chemically strengthened glass-ceramics is within the above range, indicating that the chemically strengthened glass-ceramics has a higher tensile stress level, reflecting that it has a higher surface stress level. The higher surface compressive stress level can offset more residual energy from falling, squeezing, impact or collision, thereby ensuring that it has excellent damage resistance and excellent deformation resistance.

[0192] In some embodiments of the present application, the Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 680 kgf / mm 2 Preferably, the Vickers hardness of the chemically strengthened glass-ceramics is 700 kgf / mm 2 ~800kgf / mm 2 In some embodiments, the chemically strengthened glass-ceramics has a strength of 680 kgf / mm 2 、700kgf / mm 2 、710kgf / mm 2 、720kgf / mm 2 、730kgf / mm 2 、740kgf / mm 2 、750kgf / mm 2、760kgf / mm 2 、770kgf / mm 2 、780kgf / mm 2 、790kgf / mm 2 or 800kgf / mm 2 Vickers hardness, or a Vickers hardness within a numerical range consisting of any two of the above specific values ​​as endpoints, as long as the chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. It should be understood that in a specific embodiment, any of the above ranges can be combined with any other ranges, as long as the chemically strengthened microcrystalline glass with the required performance of the present application can be obtained. The Vickers hardness of the chemically strengthened microcrystalline glass is within the above range, indicating that the chemically strengthened microcrystalline glass has a high hardness, thereby ensuring that it has excellent mechanical properties.

[0193] In the present application, those skilled in the art can select the thickness of the microcrystalline glass or chemically strengthened microcrystalline glass according to the needs. For example, the thickness of the microcrystalline glass or chemically strengthened microcrystalline glass can be 0.2mm-5mm, 0.2mm-2.0mm, 0.2mm-0.8mm, 0.4mm-0.6mm or 0.2mm-0.7mm, etc.

[0194] In the present application, by making the chemically strengthened glass-ceramics meet specific composition and stress characteristics, it can be ensured that the chemically strengthened glass-ceramics have excellent mechanical strength properties, excellent mechanical strength properties, excellent damage resistance and excellent deformation resistance.

[0195] In some embodiments of the present application, at a thickness of 0.5 mm, a 10 mm diameter round head metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened microcrystalline glass. When the center of the main surface of the chemically strengthened microcrystalline glass is subjected to a 10 kgf load, the deformation of the stress position of the chemically strengthened microcrystalline glass in the stress direction is ≤ 0.850 mm. The smaller the deformation of the chemically strengthened microcrystalline glass after being squeezed, the better its anti-deformation ability is. When it is used as the cover glass of a display screen, the smaller the deformation after being squeezed or impacted, the smaller the probability of contacting the inner screen of the glass is, which is conducive to improving the problem of failure of the inner screen of the glass caused by the impact of the cover glass. In some embodiments, at a thickness of 0.5 mm, when the center of the main surface of the chemically strengthened microcrystalline glass is subjected to a load of 10 kgf for compression, the deformation of the stress-bearing position of the chemically strengthened microcrystalline glass in the stress direction can be 0.806 mm, 0.804 mm, 0.787 mm, 0.828 mm, 0.798 mm, 0.827 mm, 0.814 mm, 0.758 mm, 0.805 mm, 0.779 mm, 0.816 mm, 0.788 mm, 0.823 mm, 0.796 mm, 0.782 mm, 0.764 mm or 0.850 mm, or a value below any of the above specific values, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0196] In some embodiments of the present application, at a thickness of 0.5 mm, a 10 mm diameter round head metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened microcrystalline glass. When the center of the main surface of the chemically strengthened microcrystalline glass undergoes a deformation of 0.400 mm along the force direction, the load borne by the center of the main surface of the chemically strengthened microcrystalline glass is ≥ 30 N. When a certain amount of deformation occurs, the greater the load that the chemically strengthened microcrystalline glass can withstand, the greater the load that can be offset by its deformation when the chemically strengthened microcrystalline glass is subjected to extrusion or impact. Therefore, when its deformation contacts the inner screen of the glass, the extrusion or impact load borne by the inner screen of the glass will be smaller, and the possibility of failure of the inner screen of the glass will be reduced. Using chemically strengthened microcrystalline glass that can withstand or offset a large load as the cover glass is conducive to improving the problem of failure of the inner screen of the glass caused by impact or extrusion of the cover glass. In some embodiments, at a thickness of 0.5 mm, a 10 mm diameter round-headed metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened microcrystalline glass. When the center of the main surface of the chemically strengthened microcrystalline glass is deformed by 0.400 mm along the force direction, the load borne by the center of the main surface of the chemically strengthened microcrystalline glass can be 36.9 N, 38.6 N, 38.5 N, 33.8 N, 37.2 N, 34.9 N, 37.4 N, 39.2 N, 38.1 N, 37.6 N, 38.7 N, 37.8 N, 38.4 N, 39.4 N or 40.0 N, or a value above any of the above specific values, or a value within the numerical range formed by any two of the above specific values ​​as endpoints.

[0197] The chemically strengthened microcrystalline glass of the present application can be obtained by subjecting the microcrystalline glass described above to chemical strengthening treatment. The chemical strengthening process can be carried out with reference to the process in the prior art, and for example, may include but is not limited to: first heating the molten salt containing a certain sodium ion concentration to the temperature required for chemical strengthening, and then preheating the microcrystalline glass (for example, a heating rate of 5°C / min-100°C / min can be used during preheating) to the required chemical strengthening temperature and then placing it in the molten salt. After constant temperature treatment until the time required for chemical strengthening is achieved, taking it out, cooling it to room temperature, cleaning the salt attached to the surface, and drying it to obtain a chemically strengthened microcrystalline glass with a high stress level and excellent deformation resistance.

[0198] In some embodiments of the present application, the temperature of the molten salt bath for chemical strengthening treatment may be 380° C.-550° C., and the time of chemical strengthening treatment may be 0.5 h-24 h.

[0199] In some embodiments of the present application, the composition of the molten salt includes 5wt%-50wt% sodium salt, 50-95wt% potassium salt and 0.01-0.30wt% lithium salt by mass ratio, and further, the selected sodium salt, potassium salt and lithium salt can be nitrate, sulfate, phosphate or carbonate, etc. In some embodiments, after the chemical strengthening treatment is completed, when the chemically strengthened microcrystalline glass is cooled, the cooling rate can be 1°C / min-50°C / min.

[0200] In the present application, the chemically strengthened microcrystalline glass prepared from the aforementioned microcrystalline glass with high strength and transparency has excellent deformation resistance and excellent drop damage resistance. When the chemically strengthened microcrystalline glass is used as the cover glass of electronic equipment, it can not only ensure that the cover glass of the electronic equipment is difficult to break, but also effectively prevent the cover glass from being squeezed or impacted, which may impact the inner screen and cause the inner screen to break or fail, thereby ensuring that the inner screen is better protected.

[0201] The transparent microcrystalline glass or chemically strengthened microcrystalline glass provided by the present application with excellent mechanical strength performance and excellent deformation resistance can be used in electronic devices, including but not limited to mobile phones, tablet computers, handheld game consoles, portable digital devices (such as digital cameras), vehicle-mounted central control, electronic whiteboard glass, smart home, and can also be used in vehicles, aircraft or aircraft, and can also be used in any glass device of microcrystalline glass required. For example, it can be used for display screens, cover glass, touch screens, glass inner screens or inner frames of electronic devices; for example, it can be used for windshields of vehicles, aircraft or aircraft, such as front windshields or side windshields. For example, it can be used for work surfaces, other surfaces, appliance doors, floor tiles, wall panels or storage containers. Other surfaces can include but are not limited to exterior wall surfaces, stair tread surfaces, column veneers or counter surfaces, etc. Storage containers can include but are not limited to cups, plates, medicine bottles or beverage bottles, etc.

[0202] The embodiments of the present application are described in detail below, which are exemplary and are only used to explain the present application, and should not be construed as limiting the present application.

[0203] In the example numbers of the following table: S refers to an embodiment, such as S1 refers to embodiment 1; D refers to a comparative example, such as D1 refers to comparative example 1.

[0204] Example 1

[0205] (1) Preparation of substrate glass:

[0206] Prepare raw materials with a total mass of 1000g (the raw materials are configured according to the formula of S1 in Table 1, and the proportions of each oxide are shown in Table 2), and add 5g of sodium chloride to the configured raw materials, mix at a speed of 25r / min in a V-type mixer for 30min, and melt in a platinum crucible at 1650℃ for 5h, then pour into a mold to form a glass brick, cool to 900℃, put into a 460℃ annealing furnace for annealing for 12h, and then cool to room temperature with the furnace to obtain a base material glass brick.

[0207] (2) Preparation of microcrystalline glass: Place the substrate glass brick in a crystallization furnace, heat the temperature from room temperature to 525°C at a rate of 10°C / min, perform nucleation treatment, keep the temperature at this temperature for 240 minutes, then heat the temperature to 685°C at a rate of 10°C / min, perform crystallization treatment, keep the temperature at this temperature for 60 minutes, and then cool it to room temperature at a rate of 1°C / min to obtain a microcrystalline glass brick. The composition of the prepared microcrystalline glass is the same as that of the substrate glass in terms of the molar percentage of oxides, see Tables 1 and 2 for details.

[0208] The obtained glass-ceramic sample bricks are cut, CNC processed (the CNC equipment model used in this application is: RCG500S), and polished in sequence to obtain glass-ceramic samples that meet the required specifications and requirements. In this application, the glass-ceramic sample bricks are subjected to the aforementioned cold processing to produce glass-ceramic samples with a thickness of 0.50 mm, specifically, glass-ceramic polished sheet samples of 50 mm×50 mm×0.5 mm.

[0209] Test results of the glass-ceramics obtained from S1:

[0210] The main crystal phase, crystallinity, average crystal size, expansion softening point, density, refractive index, Young's modulus and optical b value and transmittance (under 550nm wavelength light) of the microcrystalline glass with a thickness of 0.5mm were tested respectively, and the results are shown in Table 3.

[0211] (3) Preparation of chemically strengthened microcrystalline glass: The obtained microcrystalline glass sample is placed in the strengthening furnace cavity for preheating for 5 minutes. After preheating, it is quickly placed in a molten salt at 450°C for chemical strengthening. The composition of the molten salt is 29.99wt% NaNO3+69.98wt% KNO3+0.03wt% LiNO3. After chemical strengthening for 21.0 hours, the glass sample is taken out and placed on the strengthening furnace body to slowly cool to room temperature. The salt wrapped on the glass surface is washed off with clean water. After the glass sample is dried, the chemically strengthened microcrystalline glass can be obtained.

[0212] Test results of chemically strengthened glass-ceramics obtained from S1:

[0213] Ⅰ. The chemically strengthened microcrystalline glass was measured in an SLP 2000 (Luceo, Japan) stress meter (the light source wavelength used was 518 nm, SOC = 25.5 (nm / cm) / MPa, the refractive index was set according to the refractive index value of the microcrystalline glass sample, the refractive index of the microcrystalline glass sample in S1 was 1.5600, and the exposure time was 300 μsec), |CT_CV|, DOL_0, |CT_AV|; and then the tensile stress line density (CT_LD) value was calculated. The results are shown in Table 4.

[0214] Ⅱ. The Vickers hardness of the chemically strengthened glass-ceramics was tested. The results are shown in Table 4.

[0215] III. Test the deformation resistance of chemically strengthened microcrystalline glass, such as the deformation of chemically strengthened microcrystalline glass under a load of 10 kgf; the load borne by chemically strengthened microcrystalline glass when a deformation of 0.40 mm occurs. The results are shown in Table 4.

[0216] Example 2-Example 18

[0217] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each example are shown in Tables 1 to 4, respectively.

[0218] The DSC curve of the substrate glass of Example 3 is as follows: Figure 1 As shown, this figure can be used as a reference to determine the heat treatment process used when preparing microcrystalline glass from the substrate glass.

[0219] The XRD pattern of the glass-ceramics of Example 3 is as follows: Figure 2 As shown in the figure, it can be seen that the main crystalline phase in the microcrystalline glass is the lithium disilicate crystalline phase.

[0220] The transmittance curve of the microcrystalline glass of Example 3 is as follows: Figure 3 As shown in the figure, it can be seen that the microcrystalline glass is transparent in the visible light range and has a high transmittance.

[0221] The load deformation curve of the chemically strengthened glass-ceramics of Example 3 is as follows: Figure 4 As shown in the figure, it can be seen that the deformation of the chemically strengthened microcrystalline glass under different load extrusion, as well as the load conditions borne by the chemically strengthened microcrystalline glass when different deformations occur.

[0222] Comparative Example 1-Comparative Example 8

[0223] The above methods are respectively carried out with reference to Example 1, except that the raw material composition, different process parameters and corresponding test results of each comparative example are shown in Tables 5 to 8, respectively.

[0224] The load deformation curve of the chemically strengthened microcrystalline glass of comparative example 3 is as follows: Figure 5 shown.

[0225] Crystallization upper limit temperature test: In order to analyze the industrial mass production feasibility of the microcrystalline glass of the present application, the crystallization upper limit temperature of the substrate glass of some embodiments was tested. Among them, the crystallization upper limit temperature of the substrate glass of S3 was 1067.2°C, and the crystallization upper limit temperature of the substrate glass of S4 was 1053.5°C, both of which were lower than 1100°C. The crystallization upper limit temperature was between 1000°C and 1100°C, indicating that the microcrystalline glass of the present application is conducive to industrial mass production.

[0226] Expansion softening point test: In order to analyze the 3D hot bending effect of the microcrystalline glass of the present application, the expansion softening points of the microcrystalline glass in some embodiments were tested. See Table 3 for details. From the test results, it can be seen that the expansion softening points of the microcrystalline glass of the present application are all lower than 830°C, between 750°C and 850°C, indicating that the microcrystalline glass of the present application is conducive to 3D hot bending to prepare 3D curved microcrystalline glass.

[0227]

[0228]

[0229]

[0230]

[0231]

[0232] It can be seen from the examples of Tables 1 to 4 and the comparative examples of Tables 5 to 8 that, relative to the comparative example, the embodiment scheme of the present application not only satisfies the content range of each oxide, but also satisfies the specific oxide content relationship, and the obtained microcrystalline glass has excellent optical properties and high Young's modulus, and the lithium disilicate crystal phase is the main crystal phase of the microcrystalline glass. Moreover, the chemically strengthened microcrystalline glass obtained by using the microcrystalline glass of the embodiment of the present application can obtain high stress levels and high mechanical strength properties, and its deformation resistance is significantly better than that of the comparative example. In addition, the upper limit temperature of crystallization of the substrate glass corresponding to the microcrystalline glass of the embodiment of the present application is relatively low, indicating that it is suitable for industrial mass production. At the same time, the expansion softening point temperature of the microcrystalline glass of the embodiment of the present application is suitable, indicating that it is suitable for 3D hot bending to form 3D curved microcrystalline glass.

[0233] In the solutions of Comparative Examples 1 to 8, the glass formulas do not simultaneously satisfy: the content ranges of various oxides in the present application, and the specific oxide content relationships. The prepared microcrystalline glass either has poor optical properties, or it is impossible to prepare chemically strengthened microcrystalline glass with superior deformation resistance.

[0234] contrast Figure 4 and Figure 5 It can be seen that when the center of the main surface of the chemically strengthened microcrystalline glass of Example 3 of the present application is squeezed to produce a deformation of 0.40 mm, the load it bears or offsets is significantly greater than that of Comparative Example 3. It can be seen that the chemically strengthened microcrystalline glass of the present application has better anti-deformation ability.

[0235] The preferred embodiments of the present application are described in detail above, but the present application is not limited thereto. Within the technical concept of the present application, the technical solution of the present application can be subjected to a variety of simple modifications, including combining various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed in the present application and belong to the protection scope of the present application.

Claims

1. A glass-ceramic, characterized in that: The glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the glass-ceramics; The composition of the glass-ceramics includes, in terms of molar percentage of oxides: SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol%, MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol% , Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, Li2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%; The composition of the microcrystalline glass satisfies the following conditions, expressed in terms of the molar percentage of each oxide in the microcrystalline glass composition: 2.00≤SiO2 / Li2O≤2.40, preferably, 2.00≤SiO2 / Li2O≤2.30, and more preferably, 2.02≤SiO2 / Li2O≤2.

20.

2. The glass-ceramic according to claim 1, characterized in that: The composition of the glass-ceramics further satisfies the following conditions, measured in terms of the content of each oxide in the glass-ceramics as a molar percentage: 0.90≤SiO2+Li2O≤0.96, preferably, 0.90≤SiO2+Li2O≤0.95; and / or, Al2O3 / SiO2≤0.

030.

3. The glass-ceramic according to claim 1 or 2, characterized in that: The composition of the glass-ceramics further satisfies the following requirements, measured in terms of the content of each oxide in the glass-ceramics as a molar percentage: 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50, preferably, 0.32≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.20, more preferably, 0.36≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.10; and / or, 0.10≤ZrO2 / (100%-3×Li2O)≤0.60, preferably, 0.12≤ZrO2 / (100%-3×Li2O)≤0.52, more preferably, 0.16≤ZrO2 / (100%-3×Li2O)≤0.50; and / or, 0.034≤ZrO2 / SiO2≤0.100, preferably, 0.035≤ZrO2 / SiO2≤0.095, more preferably, 0.055≤ZrO2 / SiO2≤0.

095.

4. The glass-ceramic according to any one of claims 1 to 3, characterized in that: The composition of the glass-ceramics further satisfies the following requirements, measured in terms of the content of each oxide in the glass-ceramics as a molar percentage: CaO+Al2O3≤0.065, preferably, CaO+Al2O3≤0.055, more preferably, CaO+Al2O3≤0.050; and / or, (CaO+Al2O3) / Li2O≤0.25, preferably, (CaO+Al2O3) / Li2O≤0.20, more preferably, (CaO+Al2O3) / Li2O≤0.

14.

5. The glass-ceramic according to any one of claims 1 to 4, characterized in that: The composition of the glass-ceramics further satisfies the following requirements, measured in terms of the content of each oxide in the glass-ceramics as a molar percentage: 0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40, preferably, 0.14≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.16, more preferably, 0.50≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤3.00; and / or, Na2O / SiO2≤0.05, preferably, Na2O / SiO2≤0.04, more preferably, Na2O / SiO2≤0.

02.

6. The glass-ceramic according to any one of claims 1 to 5, characterized in that: In terms of molar percentage of oxides, the glass-ceramics comprises: The content of SiO2 is 60.00mol%-65.00mol%, preferably the content of SiO2 is 60.50mol%-64.00mol%; and / or, The content of Li2O is 28.00mol%-31.00mol%, preferably the content of Li2O is 29.00mol%-30.50mol%; and / or, The content of ZrO2 is 3.20mol%-6.00mol%, preferably the content of ZrO2 is 4.00mol%-6.00mol%; and / or, The content of P2O5 is 1.50mol%-3.00mol%, preferably the content of P2O5 is 1.50mol%-2.50mol%; and / or, The content of Na2O is 0.00mol%-1.00mol%, preferably the content of Na2O is 0.00mol%-0.50mol%; and / or, The content of CaO is 0.00 mol% to 4.00 mol%, preferably the content of CaO is 0.00 mol% to 2.50 mol%.

7. The glass-ceramic according to any one of claims 1 to 6, characterized in that: Calculated in molar percentage of oxides, the composition of the microcrystalline glass also includes: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

8. The glass-ceramic according to any one of claims 1 to 7, characterized in that: Calculated as a molar percentage of oxides, the sum of the contents of Na2O and K2O in the microcrystalline glass is less than 1.00 mol%.

9. The glass-ceramic according to any one of claims 1 to 8, characterized in that: The density of the microcrystalline glass is ρ≥2.50g / cm 3 Preferably, the density ρ of the microcrystalline glass is 2.50 g / cm 3 ~2.75g / cm 3 ; and / or, the refractive index of the microcrystalline glass is ≤1.

60.

10. The glass-ceramic according to any one of claims 1 to 9, characterized in that: The crystallinity of the glass-ceramics is 30.00wt%-90.00wt%, preferably, the crystallinity is 50.00wt%-90.00wt%, and the crystallinity is 65.00wt%-90.00wt%; and / or, In the microcrystalline glass, the average crystal size is ≤100 nm, preferably, the average crystal size is ≤50 nm, and more preferably, the average crystal size is 15 nm to 45 nm.

11. The glass-ceramic according to any one of claims 1 to 10, characterized in that: The Young's modulus of the microcrystalline glass is ≥100.00 GPa. Preferably, the Young's modulus of the microcrystalline glass is ≥110.00 GPa. More preferably, the Young's modulus of the microcrystalline glass is 114 GPa to 130 GPa.

12. The glass-ceramic according to any one of claims 1 to 11, characterized in that: At a thickness of 0.5 mm, the b value of the glass-ceramics is ≤1.0, preferably ≤0.8; and / or, The microcrystalline glass is transparent in the visible light range; at a thickness of 0.5 mm, for light of 550 nm wavelength, the transmittance of the microcrystalline glass is ≥85.00%, preferably, the transmittance of the microcrystalline glass is ≥90.00%.

13. The glass-ceramic according to any one of claims 1 to 12, characterized in that: The expansion softening point of the microcrystalline glass is 750°C to 850°C. Preferably, the expansion softening point of the microcrystalline glass is 750°C to 830°C.

14. A chemically strengthened glass-ceramic, characterized in that: The composition at the center of the chemically strengthened glass-ceramics is the same as the composition of the glass-ceramics described in any one of claims 1 to 13, and the chemically strengthened glass-ceramics includes a compressive stress layer region extending from the surface of the chemically strengthened glass-ceramics to the compression depth, and has tensile stress inside the chemically strengthened glass-ceramics.

15. The chemically strengthened glass-ceramics according to claim 14, characterized in that: The chemically strengthened glass-ceramics contains a lithium disilicate crystalline phase, wherein the lithium disilicate crystalline phase has a higher weight percentage than other crystalline phases present in the chemically strengthened glass-ceramics; in terms of molar percentage of oxides, the composition at the center of the chemically strengthened glass-ceramics includes: SiO2: 55.00mol%-65.00mol%, Al2O3: 0.00mol%-2.00mol%, P2O5: 1.00mol%-3.00mol%, ZrO2: 2.00mol%-6.00mol% , MgO: 0.00mol%-2.00mol%, ZnO: 0.00mol%-2.00mol%, Na2O: 0.00mol%-3.00mol%, K2O: 0.00mol%-1.00mol%, L i2O: 27.00mol%-32.00mol%, CaO: 0.00mol%-5.00mol%, B2O3: 0.00mol%-1.00mol%, SrO: 0.00mol%-2.00mol%; The composition at the center of the chemically strengthened glass-ceramics, expressed in terms of the content as a molar percentage of oxides, satisfies: 2.00≤SiO2 / Li2O≤2.40, preferably, 2.00≤SiO2 / Li2O≤2.30, and more preferably, 2.02≤SiO2 / Li2O≤2.

20.

16. The chemically strengthened glass-ceramics according to claim 14 or 15, characterized in that: The composition at the center of the chemically strengthened glass-ceramics further satisfies the following conditions, expressed in terms of the content expressed as a molar percentage of oxides: 0.90≤SiO2+Li2O≤0.96; and / or, Al2O3 / SiO2≤0.030; and / or, 0.31≤ZrO2 / (CaO+ZrO2+Al2O3)≤1.50; and / or, 0.10≤ZrO2 / (100%-3×Li2O)≤0.60; and / or, 0.034≤ZrO2 / SiO2≤0.100; and / or, CaO+Al2O3≤0.065; and / or, (CaO+Al2O3) / Li2O≤0.25; and / or, 0.12≤(ZrO2-Na2O) / (SiO2-2×Li2O)≤6.40; and / or, Na2O / SiO2≤0.

05.

17. The chemically strengthened glass-ceramics according to any one of claims 14 to 16, characterized in that: The composition at the center of the chemically strengthened glass-ceramics includes, in terms of molar percentage of oxides: The content of SiO2 is 60.00mol%-65.00mol%, preferably the content of SiO2 is 60.50mol%-64.00mol%; and / or, The content of Li2O is 28.00mol%-31.00mol%, preferably the content of Li2O is 29.00mol%-30.50mol%; and / or, The content of ZrO2 is 3.20mol%-6.00mol%, preferably the content of ZrO2 is 4.00mol%-6.00mol%; and / or, The content of P2O5 is 1.50mol%-3.00mol%, preferably the content of P2O5 is 1.50mol%-2.50mol%; and / or, The content of Na2O is 0.00mol%-1.00mol%, preferably the content of Na2O is 0.00mol%-0.50mol%; and / or, The content of CaO is 0.00 mol% to 4.00 mol%, preferably the content of CaO is 0.00 mol% to 2.50 mol%.

18. The chemically strengthened glass-ceramics according to any one of claims 14 to 17, characterized in that: Calculated in molar percentage of oxides, the composition at the center of the chemically strengthened glass-ceramics further includes: Y2O3: 0.00mol%-1.00mol%, La2O3: 0.00mol%-1.00mol%, Ta2O5: 0.00mol%-1.00mol%.

19. The chemically strengthened glass-ceramics according to any one of claims 14 to 18, characterized in that: The chemically strengthened glass-ceramics has a DOL_0 of 0.18t-0.25t. Preferably, the chemically strengthened glass-ceramics has a DOL_0 of 0.20t-0.25t, where DOL_0 is the depth of the compressive stress layer and t is the thickness of the chemically strengthened glass-ceramics.

20. The chemically strengthened glass-ceramics according to any one of claims 14 to 19, characterized in that: The chemically strengthened glass-ceramics has a |CT_AV| of 85MPa-200MPa. Preferably, the chemically strengthened glass-ceramics has a |CT_AV| of 90MPa-200MPa. More preferably, the chemically strengthened glass-ceramics has a |CT_AV| of 130MPa-200MPa, where |CT_AV| is the absolute value of the average tensile stress.

21. The chemically strengthened glass-ceramics according to any one of claims 14 to 20, characterized in that: The chemically strengthened glass-ceramics have a CT_LD of 50000MPa / mm-100000MPa / mm. Preferably, the chemically strengthened glass-ceramics have a CT_LD of 55000MPa / mm-100000MPa / mm. More preferably, the chemically strengthened glass-ceramics have a CT_LD of 65000MPa / mm-100000MPa / mm, where CT_LD is the tensile stress line density.

22. The chemically strengthened glass-ceramics according to any one of claims 14 to 21, characterized in that: The chemically strengthened glass-ceramics has a |CT_CV| of 120 MPa-320 MPa. Preferably, the chemically strengthened glass-ceramics has a |CT_CV| of 135 MPa-300 MPa. More preferably, the chemically strengthened glass-ceramics has a |CT_CV| of 160 MPa-300 MPa.

23. The chemically strengthened glass-ceramics according to any one of claims 14 to 22, characterized in that: The Vickers hardness of the chemically strengthened glass-ceramics is greater than or equal to 680 kgf / mm 2 Preferably, the Vickers hardness of the chemically strengthened glass-ceramics is 700 kgf / mm 2 ~800kgf / mm 2 .

24. The chemically strengthened glass-ceramics according to any one of claims 14 to 23, characterized in that: At a thickness of 0.5 mm, a 10 mm diameter round-headed metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened microcrystalline glass. When the center of the main surface of the chemically strengthened microcrystalline glass is subjected to a load of 10 kgf, the deformation of the stress position of the chemically strengthened microcrystalline glass in the stress direction is ≤0.850 mm.

25. The chemically strengthened glass-ceramics according to any one of claims 14 to 24, characterized in that: At a thickness of 0.5 mm, a 10 mm diameter round-headed metal pressure rod is used to squeeze the center of the main surface of the chemically strengthened microcrystalline glass. When the center of the main surface of the chemically strengthened microcrystalline glass undergoes a deformation of 0.400 mm along the direction of force, the load borne by the center of the main surface of the chemically strengthened microcrystalline glass is ≥30 N.

26. A glass device, characterized in that: The glass device comprises the glass-ceramics according to any one of claims 1 to 13 or comprises the chemically strengthened glass-ceramics according to any one of claims 14 to 25.

27. An electronic device, characterized in that: The electronic device comprises the glass-ceramics according to any one of claims 1 to 13 or comprises the chemically strengthened glass-ceramics according to any one of claims 14 to 25.

Citation Information

Patent Citations

  • Rare earth-mixing high strength lithium bisilicate sitall material and preparation method thereof

    CN101580343A

  • Lithium disilicate glass ceramics, method for the production thereof and use thereof

    CN102741186A

  • Zirconia-toughened glass ceramics

    CN109476532A

  • Glass ceramic with high elasticity modulus, and reinforced glass ceramic and preparation method thereof

    CN111087174A

  • Lithium disilicate microcrystalline glass suitable for rapid coloring process and preparation method thereof

    CN111908794A

Cited By

  • Glass ceramic, chemically strengthened glass ceramic and uses thereof

    WO2025162316A1

  • Microcrystalline glass, preparation method therefor and use thereof

    WO2025162318A1

  • Chemically strengthened microcrystalline glass, cover glass, electronic device, and glass device

    WO2026067725A1