Cement grinding aid and preparation method thereof

By using components such as quaternized lignin, modified nanosilicon dioxide and triethanolamine in cement aids, the problems of low efficiency and poor compressive performance of existing cement aids are solved, and more efficient Grinding and better compressive resistance.

CN118930093APending Publication Date: 2024-11-12XINJIANG KERUN TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411010966.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing cement aids are not very efficient during use, and it is difficult to effectively improve the compressive performance of cement.

Method used

Using quaternized lignin, modified nano silica, triethanolamine and thickening dispersant, cement aids are synthesized through specific preparation methods to improve the dispersion and fluidity during cement grinding and reduce the Particle agglomeration, improving grinding efficiency and compressive resistance.

Benefits of technology

It significantly improves the grinding efficiency and compressive resistance of cement, reduces particle aggregation, improves the strength and flowability of concrete, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964338710000081
    Figure BDA0004964338710000081
  • Figure BDA0004964338710000091
    Figure BDA0004964338710000091
  • Figure BDA0004964338710000092
    Figure BDA0004964338710000092
Patent Text Reader

Abstract

The invention relates to the technical field of cement, and discloses a cement grinding aid and a preparation method thereof.Quaternized lignin, modified nano-silica, triethanolamine, a thickening dispersant and water are added into a stirrer and stirred, and the cement grinding aid is obtained after stirring is finished. Lignin in the cement grinding aid improves dispersity and fluidity in the cement grinding process, so that aggregation among particles is reduced, grinding efficiency is improved, lignin can adjust charge properties of cement particles, the cement particles are repelled, agglomeration is reduced, and meanwhile lignin can further improve the strength of concrete. Wherein the nanosilicon dioxide improves the microstructure of the concrete through a filling effect and an accelerated hydration effect, has a relatively good grinding aiding effect, and also improves the compression resistance of the concrete at the same time; and the contained sulfonic acid group and quaternary ammonium salt synergistically improve the grinding efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cement, in particular to a cement grinding aid and a preparation method thereof. Background Art

[0002] Cement grinding aid is a chemical additive that improves the grinding effect and performance of cement. It is adsorbed on the surface of cement, and the hourly output of cement is increased while maintaining the fineness of the ground cement and the power of the mill unchanged. It can also reduce energy consumption and improve fluidity. At present, the raw material of cement grinding aid is still amine compounds, and the grinding efficiency is not high during use. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, patent CN103771753B discloses a cement grinding aid and a preparation method thereof, which is made of the following components in mass percentage: 36-45 parts of industrial waste liquid; 3-8 parts of amine compounds; 1-4 parts of polymerized polyols; 9-24 parts of waste sugar residues; 15-40 parts of catalysts, which reduces costs and is more environmentally friendly, but the grinding efficiency is not improved. Summary of the invention

[0003] 1. Technical issues to be resolved

[0004] In view of the deficiencies of the prior art, the present invention provides a cement grinding aid and a preparation method thereof, which has good grinding efficiency, reduces particle agglomeration, and improves the compression resistance of cement.

[0005] (II) Technical solution

[0006] To achieve the above object, the present invention provides the following technical solution: a cement grinding aid, comprising the following components by weight: 6-10 parts by weight of quaternized lignin, 8-15 parts by weight of modified nano-silicon dioxide, 7-12 parts by weight of triethanolamine, 1-2 parts by weight of a thickening dispersant, and 30-45 parts by weight of water.

[0007] Preferably, the preparation method of the quaternized lignin is:

[0008] (1) adding 2-pyrrolylcarboxylic acid to N,N-dimethylformamide solvent, stirring evenly, then adding thionyl chloride, reacting at 75-90° C. for 6-15 hours, adding acetone after the reaction to precipitate, filtering the solvent, washing with acetone, and obtaining 2-pyrrolylcarboxylic acid chloride;

[0009] (2) adding 8-15 parts by weight of lignin and 10-18 parts by weight of 2-pyrrolyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, then adding 1-2 parts by weight of pyridine catalyst, reacting at 80-110° C., and distilling under reduced pressure after reaction, washing with acetone, filtering and drying to obtain intermediate 1;

[0010] (3) adding 8-13 parts by weight of intermediate 1 and 6-9 parts by weight of sodium 3-chloro-1-hydroxypropanesulfonate to an ethanol solvent, stirring and mixing, reacting at 75-86° C. for 7-12 hours, rotating to remove the solvent, washing with petroleum ether, filtering, and drying to obtain intermediate 2;

[0011] (4) adding 1,3-bis(dimethyl)-2-propanol and pyromellitic anhydride to 1,4-dioxane, and dropping pyridine, stirring and reacting at 65-80° C. for 10-15 hours, and concentrating under reduced pressure to remove the solvent after the reaction, and then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain tertiary aminophenyl ester;

[0012] (5) adding 5-8 parts by weight of intermediate 2 and 8-13 parts by weight of tertiary aminophenyl ester to N,N-dimethylformamide solvent, adding 0.8-1 parts by weight of p-toluenesulfonic acid catalyst after dissolution, reacting for 9-16 hours, and then removing the solvent by distillation under reduced pressure, filtering and drying to obtain intermediate 3;

[0013] (6) Add N,N-dimethylformamide, 8-16 parts by weight of intermediate 3, and 7-12 parts by weight of 1-chlorododecane into the reactor, react at 95-120° C., cool to room temperature after reaction, wash with petroleum ether, and recrystallize with ethanol to obtain quaternary ammonium lignin.

[0014] Preferably, the mass ratio of 2-pyrrolidine carboxylic acid to thionyl chloride in (1) is 1:8-14.

[0015] Preferably, the reaction time in (2) is 8-14 hours.

[0016] Preferably, the mass ratio of 1,3-bis(dimethyl)-2-propanol, pyromellitic anhydride and pyridine in (4) is 1.2-1.4:1:0.02-0.04.

[0017] Preferably, the reaction temperature in (5) is 95-110°C.

[0018] Preferably, the reaction time in (6) is 20-35h.

[0019] Preferably, the preparation method of the modified nano-silicon dioxide is:

[0020] S1. 12-15 parts by weight of nano-silica are ultrasonically dispersed into a mixed solution of 14-20 parts by weight of anhydrous ethanol and 8-13 parts by weight of deionized water, mixed evenly, and then 11-15 parts by weight of γ-aminopropyltriethoxysilane are added, reacted at 75-96 ° C for 8-15h, and after the reaction, centrifuged, washed, and dried to obtain amino-modified nano-silica;

[0021] S2. Add 2-pyrrolyl chloride and amino-modified nano-silica to N,N-dimethylformamide solvent, stir and mix, continue to add triethylamine catalyst, react at 75-87°C for 10-15h, and then distill under reduced pressure, filter and dry to obtain modified nano-silica.

[0022] Preferably, the preparation method of the cement grinding aid is: adding quaternized ammonium lignin, modified nano-silicon dioxide, triethanolamine, thickening dispersant and water into a stirrer, stirring at 75-90° C. for 20-40 minutes, and obtaining the cement grinding aid after stirring.

[0023] (III) Beneficial technical effects

[0024] The invention provides a cement grinding aid by adding quaternized lignin, modified nano silicon dioxide, triethanolamine, a thickening dispersant and water into a stirrer and stirring the mixture.

[0025] The lignin in the cement grinding aid improves the dispersibility and fluidity of cement during grinding, thereby reducing the aggregation between particles and improving the grinding efficiency. The lignin can adjust the charge properties of cement particles, so that the cement particles are repelled and the generation of agglomeration is reduced. At the same time, the lignin can also improve the strength of concrete. The nano-silicon dioxide therein improves the microstructure of concrete through the filling effect and accelerated hydration, has a good grinding aid effect, and also improves the compressive performance of concrete. The large number of amide bonds contained therein have a regulating effect on the hydration process of cement, and improve its compressive strength by forming a coordination complex with calcium ions in cement. The sulfonic acid group contained therein improves the dispersibility and fluidity of the material, prevents particle agglomeration, and improves its grinding aid efficiency. The quaternary ammonium salt therein in the cement grinding aid not only improves the grinding efficiency, reduces energy consumption and improves the cement performance, but also improves the modification of the acid anhydride, and also increases the substitution degree of the quaternary ammonium salt, further improving the grinding efficiency. DETAILED DESCRIPTION

[0026] Example 1

[0027] (1) adding 2-pyrrolylcarboxylic acid to N,N-dimethylformamide solvent, stirring evenly, then adding thionyl chloride, wherein the mass ratio of 2-pyrrolylcarboxylic acid to thionyl chloride is 1:8, reacting at 75° C. for 6 h, adding acetone after the reaction to precipitate, filtering the solvent, washing with acetone, and obtaining 2-pyrrolylcarboxylic acid chloride;

[0028] (2) adding 8 parts by weight of lignin and 10 parts by weight of 2-pyrrolyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, and then adding 1 part by weight of pyridine catalyst, reacting at 80° C. for 8 h, and then distilling under reduced pressure, washing with acetone, filtering and drying to obtain intermediate 1;

[0029] (3) 8 parts by weight of intermediate 1 and 6 parts by weight of sodium 3-chloro-1-hydroxypropanesulfonate were added to an ethanol solvent, stirred and mixed, and reacted at 75° C. for 7 h. After the reaction, the solvent was removed by rotation, washed with petroleum ether, filtered, and dried to obtain intermediate 2;

[0030] (4) adding 1,3-bis(dimethyl)-2-propanol and pyromellitic anhydride to 1,4-dioxane, and then dropping pyridine, wherein the mass ratio of 1,3-bis(dimethyl)-2-propanol, pyromellitic anhydride, and pyridine is 1.2:1:0.02, stirring and reacting at 65° C. for 10 h, and after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain tertiary aminophenyl ester;

[0031] (5) 5 parts by weight of intermediate 2 and 8 parts by weight of tertiary aminophenyl ester were added to N,N-dimethylformamide solvent, and after dissolution, 0.8 parts by weight of p-toluenesulfonic acid catalyst was added, and the reaction was carried out at 95° C. for 9 hours. After the reaction, the solvent was removed by distillation under reduced pressure, and the mixture was filtered and dried to obtain intermediate 3;

[0032] (6) Add N,N-dimethylformamide, 8 parts by weight of intermediate 3, and 7 parts by weight of 1-chlorododecane to the reactor, react at 95° C. for 20 hours, cool to room temperature after reaction, wash with petroleum ether, and recrystallize with ethanol to obtain quaternary ammonium lignin;

[0033] (7) ultrasonically dispersing 12 parts by weight of nano-silica into a mixed solution of 14 parts by weight of anhydrous ethanol and 8 parts by weight of deionized water, and after mixing evenly, adding 11 parts by weight of γ-aminopropyltriethoxysilane, reacting at 75° C. for 8 h, and after the reaction, centrifuging, washing, and drying to obtain amino-modified nano-silica;

[0034] (8) Add 2-pyrrolyl chloride and amino-modified nano-silica to N,N-dimethylformamide solvent, stir and mix, continue to add triethylamine catalyst, react at 75° C. for 10 h, and then perform reduced pressure distillation, filter and dry to obtain modified nano-silica.

[0035] (9) 6 parts by weight of quaternized lignin, 8 parts by weight of modified nano-silica, 7 parts by weight of triethanolamine, 1 part by weight of a thickening dispersant, and 30 parts by weight of water are added into a stirrer and stirred at 75° C. for 20 min to obtain a cement grinding aid.

[0036] Example 2

[0037] (1) adding 2-pyrrolylcarboxylic acid to N,N-dimethylformamide solvent, stirring evenly, then adding thionyl chloride, wherein the mass ratio of 2-pyrrolylcarboxylic acid to thionyl chloride is 1:14, reacting at 90° C. for 15 h, adding acetone after the reaction to precipitate, filtering the solvent, washing with acetone, and obtaining 2-pyrrolylcarboxylic acid chloride;

[0038] (2) adding 15 parts by weight of lignin and 18 parts by weight of 2-pyrrolyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, and then adding 2 parts by weight of pyridine catalyst, reacting at 110° C. for 14 h, and then distilling under reduced pressure, washing with acetone, filtering and drying to obtain intermediate 1;

[0039] (3) 13 parts by weight of intermediate 1 and 9 parts by weight of sodium 3-chloro-1-hydroxypropanesulfonate were added to an ethanol solvent, stirred and mixed, and reacted at 86° C. for 12 h. After the reaction, the solvent was removed by rotation, washed with petroleum ether, filtered, and dried to obtain intermediate 2;

[0040] (4) adding 1,3-bis(dimethyl)-2-propanol and pyromellitic anhydride to 1,4-dioxane, and then dropping pyridine, wherein the mass ratio of 1,3-bis(dimethyl)-2-propanol, pyromellitic anhydride, and pyridine is 1.4:1:0.04, stirring and reacting at 80° C. for 15 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain tertiary aminophenyl ester;

[0041] (5) 8 parts by weight of intermediate 2 and 13 parts by weight of tertiary aminophenyl ester were added to N,N-dimethylformamide solvent, and after dissolution, 1 part by weight of p-toluenesulfonic acid catalyst was added, and the reaction was carried out at 110° C. for 16 hours. After the reaction, the solvent was distilled off under reduced pressure, filtered and dried to obtain intermediate 3;

[0042] (6) Add N,N-dimethylformamide, 16 parts by weight of intermediate 3, and 12 parts by weight of 1-chlorododecane to the reactor, react at 120° C. for 35 hours, cool to room temperature after reaction, wash with petroleum ether, and recrystallize with ethanol to obtain quaternary ammonium lignin;

[0043] (7) ultrasonically dispersing 15 parts by weight of nano-silica into a mixed solution of 20 parts by weight of anhydrous ethanol and 13 parts by weight of deionized water, and after mixing evenly, adding 15 parts by weight of γ-aminopropyltriethoxysilane, reacting at 96° C. for 15 h, and after the reaction, centrifuging, washing, and drying to obtain amino-modified nano-silica;

[0044] (8) Add 2-pyrrolyl chloride and amino-modified nano-silica to N,N-dimethylformamide solvent, stir and mix, continue to add triethylamine catalyst, react at 87° C. for 15 h, and then perform reduced pressure distillation, filter and dry to obtain modified nano-silica.

[0045] (9) 10 parts by weight of quaternized lignin, 15 parts by weight of modified nano-silica, 12 parts by weight of triethanolamine, 2 parts by weight of a thickening dispersant, and 45 parts by weight of water are added into a stirrer and stirred at 90° C. for 40 minutes to obtain a cement grinding aid.

[0046] Example 3

[0047] (1) adding 2-pyrrolylcarboxylic acid to N,N-dimethylformamide solvent, stirring evenly, then adding thionyl chloride, wherein the mass ratio of 2-pyrrolylcarboxylic acid to thionyl chloride is 1:11, reacting at 82.5° C. for 10.5 h, adding acetone after the reaction to precipitate, filtering the solvent, washing with acetone, and obtaining 2-pyrrolylcarboxylic acid chloride;

[0048] (2) adding 11.5 parts by weight of lignin and 14 parts by weight of 2-pyrrolyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, and then adding 1.5 parts by weight of pyridine catalyst, reacting at 95° C. for 11 hours, and then distilling under reduced pressure, washing with acetone, filtering and drying to obtain intermediate 1;

[0049] (3) 10.5 parts by weight of intermediate 1 and 7.5 parts by weight of sodium 3-chloro-1-hydroxypropanesulfonate were added to an ethanol solvent, stirred and mixed, and reacted at 80.5° C. for 9.5 hours. After the reaction, the solvent was removed by rotation, washed with petroleum ether, filtered, and dried to obtain intermediate 2;

[0050] (4) adding 1,3-bis(dimethyl)-2-propanol and pyromellitic anhydride to 1,4-dioxane, and then dropping pyridine, wherein the mass ratio of 1,3-bis(dimethyl)-2-propanol, pyromellitic anhydride, and pyridine is 1.3:1:0.03, stirring and reacting at 72.5° C. for 12.5 hours, and after the reaction, concentrating under reduced pressure to remove the solvent, then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain tertiary aminophenyl ester;

[0051] (5) 6.5 parts by weight of intermediate 2 and 10.5 parts by weight of tertiary aminophenyl ester were added to N,N-dimethylformamide solvent, and after dissolution, 0.9 parts by weight of p-toluenesulfonic acid catalyst was added, and the reaction was carried out at 102.5° C. for 12.5 hours. After the reaction, the solvent was removed by distillation under reduced pressure, and the mixture was filtered and dried to obtain intermediate 3;

[0052] (6) Add N,N-dimethylformamide, 12 parts by weight of intermediate 3, and 8.5 parts by weight of 1-chlorododecane to the reactor, react at 107.5° C. for 27.5 hours, cool to room temperature after reaction, wash with petroleum ether, and recrystallize with ethanol to obtain quaternary ammonium lignin;

[0053] (7) ultrasonically dispersing 13.5 parts by weight of nano-silica into a mixed solution of 17 parts by weight of anhydrous ethanol and 10.5 parts by weight of deionized water, and after mixing evenly, adding 13 parts by weight of γ-aminopropyltriethoxysilane, reacting at 50.5° C. for 11.5 hours, and after the reaction, centrifuging, washing, and drying to obtain amino-modified nano-silica;

[0054] (8) Add 2-pyrrolyl chloride and amino-modified nano-silica to N,N-dimethylformamide solvent, stir and mix, continue to add triethylamine catalyst, react at 81° C. for 12.5 hours, and then perform vacuum distillation, filter and dry to obtain modified nano-silica.

[0055] (9) 8 parts by weight of quaternized lignin, 11.5 parts by weight of modified nano-silica, 9.5 parts by weight of triethanolamine, 1.5 parts by weight of a thickening dispersant, and 37.5 parts by weight of water were added into a stirrer and stirred at 82.5° C. for 30 min to obtain a cement grinding aid.

[0056] Comparative Example 1

[0057] (1) 11.5 parts by weight of modified nano-silicon dioxide, 9.5 parts by weight of triethanolamine, 1.5 parts by weight of a thickening dispersant, and 37.5 parts by weight of water were added into a stirrer and stirred at 82.5° C. for 30 minutes to obtain a cement grinding aid.

[0058] Comparative Example 2

[0059] (1) 8 parts by weight of quaternized lignin, 9.5 parts by weight of triethanolamine, 1.5 parts by weight of a thickening dispersant, and 37.5 parts by weight of water were added into a stirrer and stirred at 82.5° C. for 30 min to obtain a cement grinding aid.

[0060] The cement grinding aids of Examples 1-3 and Comparative Examples 1-2 of the present invention were made into 18 wt % aqueous solution, and 0.03 wt % was added and evenly sprayed on the surface of the cement material to be ground. The cement was ground for 15 min and the specific surface area was tested. The test results are shown in Table 1.

[0061] Table 1: Grinding aids tested.

[0062]

[0063]

[0064] It can be seen from Table 1 that the specific surface area of ​​cement particles in Examples 1-3 of the present invention is larger than that in Comparative Examples 1-2.

[0065] The strength test of the cement after grinding of Examples 1-3 and Comparative Examples 1-2 was carried out, specifically in accordance with the provisions of GB175-2007 "General Portland Cement", the method specified in GB / T17671-1999 "Test Method for Strength of Cement Mortar (ISO Method)" was adopted, cement, standard sand and water were made into 40mm×40mm×160mm standard test pieces in a ratio of 1:3.0:0.5, and cured to the specified age under standard curing conditions (20±1℃ and relative humidity of more than 90% in air within 1d, and 20±1℃ in water after 1d), and the 3d and 28d compressive strengths were measured according to the specified methods, respectively. The test results are shown in Table 2.

[0066] Table 2: Cement strength test.

[0067]

[0068]

[0069] It can be seen from Table 2 that the cement grinding aid of the present invention, Examples 1-3 of the present invention have better compressive strength than Comparative Examples 1-2.

[0070] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A cement grinding aid, It is characterized in that The invention comprises the following components by weight: 6-10 parts by weight of quaternized lignin, 8-15 parts by weight of modified nano silicon dioxide, 7-12 parts by weight of triethanolamine, 1-2 parts by weight of thickening dispersant and 30-45 parts by weight of water.

2. The cement grinding aid according to claim 1, It is characterized in that The preparation method of the quaternized lignin is: (1) adding 2-pyrrolylcarboxylic acid to N,N-dimethylformamide solvent, stirring evenly, then adding thionyl chloride, reacting at 75-90° C. for 6-15 hours, adding acetone after the reaction to precipitate, filtering the solvent, washing with acetone, and obtaining 2-pyrrolylcarboxylic acid chloride; (2) adding 8-15 parts by weight of lignin and 10-18 parts by weight of 2-pyrrolyl chloride to N,N-dimethylformamide solvent, stirring to dissolve, then adding 1-2 parts by weight of pyridine catalyst, reacting at 80-110° C., and distilling under reduced pressure after reaction, washing with acetone, filtering and drying to obtain intermediate 1; (3) adding 8-13 parts by weight of intermediate 1 and 6-9 parts by weight of sodium 3-chloro-1-hydroxypropanesulfonate to an ethanol solvent, stirring and mixing, reacting at 75-86° C. for 7-12 hours, rotating to remove the solvent, washing with petroleum ether, filtering, and drying to obtain intermediate 2; (4) adding 1,3-bis(dimethyl)-2-propanol and pyromellitic anhydride to 1,4-dioxane, and dropping pyridine, stirring and reacting at 65-80° C. for 10-15 hours, and concentrating under reduced pressure to remove the solvent after the reaction, and then washing the crude product with ether, and then dissolving the product in dichloromethane for recrystallization and purification to obtain tertiary aminophenyl ester; (5) adding 5-8 parts by weight of intermediate 2 and 8-13 parts by weight of tertiary aminophenyl ester to N,N-dimethylformamide solvent, adding 0.8-1 parts by weight of p-toluenesulfonic acid catalyst after dissolution, reacting for 9-16 hours, and then removing the solvent by distillation under reduced pressure, filtering and drying to obtain intermediate 3; (6) Add N,N-dimethylformamide, 8-16 parts by weight of intermediate 3, and 7-12 parts by weight of 1-chlorododecane into the reactor, react at 95-120° C., cool to room temperature after reaction, wash with petroleum ether, and recrystallize with ethanol to obtain quaternary ammonium lignin.

3. The cement grinding aid according to claim 2, It is characterized in that The mass ratio of 2-pyrrolidine carboxylic acid to thionyl chloride in (1) is 1:8-14.

4. The cement grinding aid according to claim 2, It is characterized in that The reaction time in (2) is 8-14h.

5. The cement grinding aid according to claim 2, It is characterized in that The mass ratio of 1,3-bis(dimethyl)-2-propanol, pyromellitic anhydride and pyridine in (4) is 1.2-1.4:1:0.02-0.

04.

6. The cement grinding aid according to claim 2, It is characterized in that The reaction temperature in (5) is 95-110°C.

7. The cement grinding aid according to claim 2, It is characterized in that The reaction time in (6) is 20-35h.

8. The cement grinding aid according to claim 1, It is characterized in that The preparation method of the modified nano silicon dioxide is: S1. 12-15 parts by weight of nano-silica are ultrasonically dispersed into a mixed solution of 14-20 parts by weight of anhydrous ethanol and 8-13 parts by weight of deionized water, mixed evenly, and then 11-15 parts by weight of γ-aminopropyltriethoxysilane are added, reacted at 75-96 ° C for 8-15h, and after the reaction, centrifuged, washed, and dried to obtain amino-modified nano-silica; S2. Add 2-pyrrolyl chloride and amino-modified nano-silica to N,N-dimethylformamide solvent, stir and mix, continue to add triethylamine catalyst, react at 75-87°C for 10-15h, and then distill under reduced pressure, filter and dry to obtain modified nano-silica.

9. A method for preparing a cement grinding aid according to any one of claims 1 to 8, It is characterized in that The preparation method of the cement grinding aid is as follows: adding quaternized ammonium lignin, modified nano silicon dioxide, triethanolamine, thickening dispersant and water into a stirrer, stirring at 75-90° C. for 20-40 minutes, and obtaining the cement grinding aid after stirring.

Citation Information

Cited By

  • Concrete preparation method based on construction waste

    CN120903898A

  • A method for preparing concrete based on construction waste

    CN120903898B