Method for improving compressive strength of semi-hydrated ardealite cementing material, semi-hydrated ardealite cementing material and preparation method of semi-hydrated ardealite cementing material
By using sulfate-containing ion solution in phosphogypsum gelling materials for curing, the problems of low dosage and poor mechanical properties of phosphogypsum gelling materials are solved, and high-strength phosphogypsum gelling materials are realized, meeting the high standard number The compressive strength requirements of cement and reduce cement use and carbon emissions.
Patent Information
- Application Number
- CN202411015637.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
The existing phosphogypsum-based gelling materials have low phosphogypsum dosage, poor working and mechanical properties, making it difficult to meet the compressive strength requirements of high-grade cements.
After the phosphogypsum gelling material is formed, the sulfate-containing ion solution is used for curing. The incompletely hydrated semi-hydrate phosphogypsum and the incompletely hydrated slag are further hydrated through the sulfate ion solution to form ettringite, reducing the system Porosity, improve mechanical strength.
The compressive strength of the gelling material with large amounts of phosphogypsum has been improved, so that the dosage of phosphogypsum reaches 70%-90%, and can reach more than 39.8MPa after 56 days of curing in sulfate solution, meeting the national standard requirements and reducing the use of cement and carbon emissions.
Smart Images

Figure CN118930096A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of building materials, and in particular to a method for improving the compressive strength of a semi-hydrated phosphogypsum cementitious material, a semi-hydrated phosphogypsum cementitious material and a preparation method thereof. Background Art
[0002] Phosphogypsum is an industrial waste discharged during the wet production of phosphoric acid. It is usually black-gray or off-white in appearance. Its main components are calcium sulfate and its hydration products, of which CaSO 4 ·2H 2O accounts for a large proportion, in addition to which it also contains impurities such as phosphide, fluoride and organic matter. In recent years, the average annual emission of phosphogypsum in China has exceeded 70 million tons. Due to insufficient comprehensive resource utilization, a large amount of phosphogypsum has been stored. A large amount of phosphogypsum not only occupies land resources, but also contains water-soluble phosphorus pentoxide and water-soluble fluorine, which seriously threaten the safety of the water environment. There are great ecological and environmental safety hazards. It is necessary to broaden the utilization of phosphogypsum and continue to promote the use of phosphogypsum in new building materials and other fields. A series of shortcomings of phosphogypsum include phosphorus and fluorine organic impurities, poor gelling properties, low strength, poor water resistance, and insufficient early strength, which will have an adverse effect on the strength and water resistance of phosphogypsum-based cementitious materials, which will restrict the application of phosphogypsum-based cementitious materials to a certain extent. The existing methods for the utilization of phosphogypsum solid waste limit its large-scale application because of its low added value, limited incorporation, or unsolidified toxic substances. It is generally used as a cement retarder or concrete admixture, and its strength does not meet the national standard requirements of high-grade cement. Among the prior art, Xie Boyin (CN 111362601 A) discloses a high-dosage phosphogypsum cement clinker cementitious material and a preparation method thereof, wherein the high-dosage phosphogypsum formula is 52wt% phosphogypsum, 23% cement, 8% phosphorus slag powder, 17% fly ash, and 1.5% powdered phosphorus activator mixed and ground, and 0.6% aqueous phosphorus activator is added to obtain a high-dosage phosphogypsum-based cementitious material, and after curing for 28 days, its compressive strength can reach up to 39.68MPa, reaching the standard of 32.5 cement. Yang Wen (CN 111792902 A) discloses a high-strength water-resistant phosphogypsum composite cementitious material and a preparation method thereof, wherein the phosphogypsum used is β-type phosphogypsum, which needs to be pretreated at high temperature to be obtained, and a variety of organic waterproofing agents are added therein, and its compressive strength reaches up to 45MPa, reaching the national standard requirement of 42.5 cement. Tan Hongbo (CN 114933427A) disclosed a method for preparing low-carbon cement based on industrial solid waste, in which the solid waste phosphogypsum content is only 2-5wt%, and high temperature treatment is required. Sun Zhengping (CN 106747186 A) disclosed a concrete curbstone prepared with phosphogypsum-based hydraulic composite cementitious material and its preparation method, in which blast furnace slag is the main component, accounting for more than 50%, and the kaolin content is relatively low, the alkali activator is only water glass, and the mechanical strength is mainly generated by the volcanic ash effect of the slag. The components of limestone, kaolin, CaF 2It is mainly used for setting and does not participate in the formation of mechanical strength. Wan Xinlong applied phosphogypsum to slag-metakaolin polymer in the literature (Application of phosphogypsum in slag-metakaolin polymer), with the maximum addition amount of 30wt%. In this system, phosphogypsum needs to be pretreated at high temperature. Sun Tao applied phosphogypsum to slag-cement-metakaolin in the literature (An eco-friendly phosphogypsum-based cementitous materials: performance optimization and enhancing mechanisms), with the maximum addition amount of 45%. The strength of this system is mainly formed by the reaction of slag and phosphogypsum to form calcium sulfonate, and the material needs to be adjusted to pH 11.8 through a wet grinding process. Its 3-day strength is only about 11Mpa, which does not meet the national standard for cement application. In another paper (Recycling utilization of phosphogypsum eco excess-sulphate cement: Synergistic effects of metakaolin and slag additives onhydration, strength and microstructure), it is mentioned that the strength formation mechanism of slag and metakaolin in this system is that slag and phosphogypsum form calcium sulfonate under the action of metakaolin, and cement, due to its small addition amount, plays the role of adjusting the pH value in this system.
[0003] Therefore, it is necessary to solve the problems of low phosphogypsum content, poor working performance and mechanical properties of existing phosphogypsum-based cementitious materials, and to improve the compressive strength of phosphogypsum-based cementitious materials. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method for improving the compressive strength of a semi-hydrated phosphogypsum cementitious material, a semi-hydrated phosphogypsum cementitious material and a preparation method thereof, so as to overcome the problems of low phosphogypsum content, poor working performance and mechanical properties of existing phosphogypsum-based cementitious materials. The preparation method of this material is simple, and it has sufficient mechanical properties so that the matrix can effectively achieve late stability.
[0005] The method for improving the compressive strength of a semi-hydrated phosphogypsum cementitious material of the present invention comprises curing the phosphogypsum cementitious material with a sulfate ion-containing solution after molding to improve the compressive strength;
[0006] Furthermore, the phosphogypsum cementitious material is soaked in a sulfate ion-containing solution after being formed.
[0007] The present invention also discloses a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage, wherein the raw materials include 70-90 parts of semi-hydrated phosphogypsum, 10-30 parts of industrial granulated blast furnace slag, 30-40 parts of alkali activator, and 2-10 parts of sulfate ion-containing solution in parts by weight;
[0008] Further, the sulfate ion-containing solution is a sulfate solution;
[0009] Further, the sulfate ion-containing solution is a 5% by mass sodium sulfate solution;
[0010] Furthermore, the hemihydrate phosphogypsum is prepared by calcining phosphogypsum at high temperature;
[0011] Furthermore, the alkaline activator comprises water glass, sodium hydroxide and water, wherein the water glass comprises 0.3-0.5 parts and the sodium hydroxide comprises 0.5-0.8 parts by weight.
[0012] The present invention also discloses a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage, comprising the following steps: soaking a semi-hydrated phosphogypsum-based cementitious material prepared from semi-hydrated phosphogypsum, industrial granulated blast furnace slag and an alkali activator in a sulfate ion-containing solution after forming;
[0013] Further, the method comprises the following steps: (1) uniformly stirring and mixing an alkali activator, hemihydrate phosphogypsum and industrial granulated blast furnace slag to prepare a cementitious material;
[0014] (2) After the cementitious material has been cured and formed, it is immersed in a solution containing sulfate ions.
[0015] The invention has the following beneficial effects: the method for improving the compressive strength of a semi-hydrated phosphogypsum cementitious material, the semi-hydrated phosphogypsum cementitious material and the preparation method thereof, by using a sulfate ion-containing solution as a curing agent for the semi-hydrated phosphogypsum cementitious material, the sulfate ions can greatly improve the compressive strength of a high-dosage phosphogypsum-based cementitious material, in the sulfate ion solution, the semi-hydrated phosphogypsum that is not completely hydrated is further hydrated, and at the same time, the residual calcium oxide is hydrated to release calcium ions and the content of hydroxide ions rapidly rises until saturation, and in a saturated alkaline environment, aluminum oxide and silicon oxide in the incompletely hydrated slag are fully precipitated to form hydrated calcium silicate and hydrated calcium aluminate with the calcium ions, and at the same time, the hydrated calcium aluminate can be further converted into ettringite due to the addition of the sulfate ion solution, so that an interwoven mesh structure is formed inside, the hydrated calcium silicate fills the internal pores, the porosity of the phosphogypsum-based cementitious material is effectively reduced, the mechanical strength of the high-dosage phosphogypsum cementitious material is improved, and the phosphogypsum dosage can reach 70%-90%. The compressive strength of the cementitious material with 90% phosphogypsum added can reach more than 39.8 MPa after curing in the sulfate solution for 56 days. Therefore, in the formula of the present invention, the immersion in the sulfate solution plays a role in further hydrating the incompletely hydrated hemihydrate phosphogypsum and the incompletely hydrated slag to form ettringite, reducing the porosity of the system and improving the strength of the cementitious material with a large amount of phosphogypsum added. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0017] Figure 1 The XRD diagram of the high-strength hemihydrate phosphogypsum cementitious material prepared in Example 6 after immersion for 28 days;
[0018] Figure 2 The XRD diagram of the high-strength hemihydrate phosphogypsum cementitious material 56d prepared in Example 6 with a large dosage;
[0019] Figure 3 The XRD pattern of the high-strength hemihydrate phosphogypsum cementitious material prepared in large dosage in Example 6 after 28 days of molding;
[0020] Figure 4 This is the EDS graph of the high-strength hemihydrate phosphogypsum cementitious material prepared in Example 6 after immersion for 56 days;
[0021] Figure 5 This is the SEM image of the high-strength hemihydrate phosphogypsum cementitious material prepared in Example 6 after 28 days of molding;
[0022] Figure 6 SEM image of high-strength hemihydrate phosphogypsum cementitious material with large dosage prepared after immersion for 56 days. DETAILED DESCRIPTION
[0023] In the method for improving the compressive strength of the hemihydrate phosphogypsum cementitious material of the present embodiment, the phosphogypsum cementitious material is cured with a sulfate ion-containing solution after being formed to improve the compressive strength; the immersion in the sulfate solution serves to further hydrate the incompletely hydrated hemihydrate phosphogypsum and the incompletely hydrated slag to form calcium sulfate, thereby reducing the porosity of the system and improving the strength of the high-dosage phosphogypsum cementitious material.
[0024] In this embodiment, the phosphogypsum cementitious material is immersed in a sulfate ion-containing solution after being formed, and the post-forming curing can be carried out by spraying the sulfate ion-containing solution.
[0025] The present embodiment also discloses a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by weight, 70-90 parts of semi-hydrated phosphogypsum, 10-30 parts of industrial granulated blast furnace slag, 30-40 parts of alkali activator, and 2-10 parts of sulfate ion solution; the sulfate ion solution is a sulfate solution; the sulfate ion solution is a 5% by mass sodium sulfate solution, and other sulfate solutions can also be used to achieve the purpose of the invention; the semi-hydrated phosphogypsum is prepared by calcining phosphogypsum at a high temperature; the alkali activator includes water glass, sodium hydroxide and water, by weight, 0.3-0.5 parts of water glass and 0.5-0.8 parts of sodium hydroxide; the cementitious material is prepared by mixing a large amount of semi-hydrated phosphogypsum with industrial granulated blast furnace slag, without adding cement clinker, and the mechanical strength is improved by soaking in sulfate. In the sulfate solution, the incompletely hydrated hemihydrated phosphogypsum is further hydrated, and the calcium ions and hydroxide ions are released, and the content rises rapidly until saturation. In the saturated alkaline environment, the alumina and silicon oxide in the incompletely hydrated slag are fully precipitated to form hydrated calcium silicate and hydrated calcium aluminate with the calcium ions. At the same time, because the sulfate solution supplements a large amount of sulfate ions, the hydrated calcium aluminate can be further converted into calcium aluminate, so that an interwoven mesh structure is formed inside, and the hydrated calcium silicate fills the internal pores, effectively reducing the porosity of the phosphogypsum-based cementitious material, and improving the mechanical strength of the high-dosage phosphogypsum cementitious material, so that the phosphogypsum dosage can reach 70%-90%. The phosphogypsum-based cementitious material not only greatly reduces the use of cement and reduces carbon emissions, but also utilizes industrial solid waste to prepare a material invention with mechanical strength that meets national standards and is suitable for production and life.
[0026] Sulfate solution immersion has a very unexpected and significant beneficial effect on improving the mechanical strength of high-volume phosphogypsum-based cementitious material systems. During the hydration reaction of 90 parts of phosphogypsum and 10 parts of slag powder under the action of an alkali activator, the compressive strength is 8 MPa after 28 days of conventional air curing. The present invention was initially intended to study the negative impact of sulfate erosion on phosphogypsum cementitious materials. It was unexpectedly found that sulfate solution curing can greatly improve the compressive strength of high-dosage phosphogypsum-based cementitious materials by immersion in sulfate solution. In the sulfate solution, the incompletely hydrated hemihydrated phosphogypsum is further hydrated, and the residual calcium oxide is hydrated to release calcium ions and the content of hydroxide ions rises rapidly until saturation. In a saturated alkaline environment, the aluminum oxide and silicon oxide in the incompletely hydrated slag are fully precipitated to form hydrated calcium silicate and hydrated calcium aluminate with calcium ions. At the same time, since the sulfate solution supplements a large amount of sulfate ions, the hydrated calcium aluminate can be further converted into calcium sulfonate, so that an interwoven network structure is formed inside, and the hydrated calcium silicate fills the internal pores, effectively reducing the porosity of the phosphogypsum-based cementitious materials, improving the mechanical strength of the high-dosage phosphogypsum cementitious materials, and making the phosphogypsum dosage reach 70%-90%. The compressive strength of the cementitious material with 90% phosphogypsum added can reach 39.8 MPa after curing in the sulfate solution for 56 days. Therefore, in the formula of the present invention, the immersion in the sulfate solution plays a role in further hydrating the incompletely hydrated hemihydrate phosphogypsum and the incompletely hydrated slag to form ettringite, reducing the porosity of the system and improving the strength of the cementitious material with a large amount of phosphogypsum added.
[0027] The present invention only uses phosphogypsum and slag powder. The simple phosphogypsum and slag powder have the problem of low ettringite generation under alkali excitation, and high content of monosulfur ettringite leading to low compressive strength. In the process of sulfate erosion experiment, it is surprisingly found that immersion in sulfate solution can greatly improve the compressive strength of cementitious materials in a large-amount phosphogypsum system. After immersion in 5% sodium sulfate solution for 56 days, the compressive strength of cementitious materials in a 90% phosphogypsum-slag powder system is improved from 8MPa to 39.8MPa; after immersion in 5% sodium sulfate solution for 56 days, the compressive strength of cementitious materials in an 80% phosphogypsum-slag powder system is improved from 21.9MPa to 49MPa; after immersion in 5% sodium sulfate solution for 56 days, the compressive strength of cementitious materials in a 70% phosphogypsum-slag powder system is improved from 24.7MPa to 53.4MPa.
[0028] The beneficial effects of using sulfate solution to soak large amounts of phosphogypsum-slag powder cementitious materials are as follows:
[0029] XRD data analysis shows that in the high-dosage phosphogypsum-based cementitious material system, a large amount of CaSO 4 This makes Al 3+Unable to communicate with sufficient SO 4 2- Combined to form ettringite, which in turn forms monosulfide ettringite with lower strength and adheres to the surface of the generated gypsum to prevent the growth of gypsum crystals. Therefore, the diffraction peak of ettringite is weak and of lower intensity at 28 days. After being immersed in sodium sulfate solution, due to the addition of a large amount of free SO 4 2- , so that the generated monosulfide type calcium sulfonate can be further converted into calcium sulfonate. At the same time, due to the addition of water, the incompletely hydrated phosphogypsum and slag can be further hydrated, which makes the CaSO 4 The content is reduced, the sample is more stable and Si 4+ and Al 3+ The content of further increases with the completion of hydration of slag, thus forming calcium sulfonate and CSH gel, which promotes the strength development of the sample. At the same time, the increase of hydration products makes the interior of the sample denser, and the sample acquires good resistance to sulfate corrosion.
[0030] The beneficial effects of high-dosage phosphogypsum-based cementitious material systems are as follows.
[0031] (1) In the early stage of the reaction, due to the high content of phosphogypsum, a large amount of CaSO is generated in the early stage of the reaction. 4 , and at the same time inhibit the formation of ettringite, so that the sample has better sulfate resistance.
[0032] (2) Due to the presence of unhydrated slag and monosulfide ettringite, the sample will preferentially release free SO 4 2- It reacts with the monosulfide ettringite formed earlier to transform into ettringite and generate a large amount of CSH gel, ensuring the strength of the phosphogypsum-based cementitious material system with a large amount of gel.
[0033] (3) The addition amount of phosphogypsum reaches 70%-90%, which can consume a large amount of phosphogypsum storage, reduce land resource occupation, reduce cement use, and effectively reduce carbon emissions and energy consumption.
[0034] This embodiment also discloses a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage, comprising the following steps: soaking a semi-hydrated phosphogypsum-based cementitious material prepared from semi-hydrated phosphogypsum, industrial granulated blast furnace slag and an alkali activator in a sulfate ion-containing solution after forming;
[0035] In this embodiment, the steps include: (1) uniformly stirring and mixing an alkali activator, hemihydrate phosphogypsum and industrial granulated blast furnace slag to prepare a cementitious material;
[0036] (2) After the cementitious material is cured and formed, it is immersed in a solution containing sulfate ions; the preparation process is simple.
[0037] Embodiment 1
[0038] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 90 parts of semi-hydrated phosphogypsum, 10 parts of industrial granulated blast furnace slag, 0.5 parts of water glass, 0.5 parts of sodium hydroxide, 32 parts of water, and 2 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding, the material is immersed in a sodium sulfate solution for 28 days and 56 days, and then a mechanical strength test is carried out.
[0039]
[0040] Embodiment 2
[0041] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 80 parts of semi-hydrated phosphogypsum, 20 parts of industrial granulated blast furnace slag, 0.5 parts of water glass, 0.5 parts of sodium hydroxide, 32 parts of water, and 10 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding and curing for 28 days, the material is immersed in a sulfate solution for 28 days and 56 days, and then a mechanical strength test is performed.
[0042]
[0043] Embodiment 3
[0044] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 70 parts of semi-hydrated phosphogypsum, 30 parts of industrial granulated blast furnace slag, 0.5 parts of water glass, 0.5 parts of sodium hydroxide, 32 parts of water, and 5 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding and curing for 28 days, the material is immersed in a sulfate solution for 28 days and 56 days, and then a mechanical strength test is performed.
[0045]
[0046] Embodiment 4
[0047] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 90 parts of semi-hydrated phosphogypsum, 10 parts of industrial granulated blast furnace slag, 0.3 parts of water glass, 0.7 parts of sodium hydroxide, 32 parts of water, and 3 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding and curing for 28 days, the material is immersed in a sulfate solution for 28 days and 56 days, and then a mechanical strength test is performed.
[0048]
[0049] Embodiment 5
[0050] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 80 parts of semi-hydrated phosphogypsum, 20 parts of industrial granulated blast furnace slag, 0.3 parts of water glass, 0.7 parts of sodium hydroxide, 32 parts of water, and 7 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding and curing for 28 days, the material is immersed in a sulfate solution for 28 days and 56 days, and then a mechanical strength test is performed.
[0051]
[0052] Embodiment 6
[0053] The present embodiment provides a method for preparing a high-strength semi-hydrated phosphogypsum cementitious material with a large dosage. The raw materials include, by mass, 70 parts of semi-hydrated phosphogypsum, 30 parts of industrial granulated blast furnace slag, 0.3 parts of water glass, 0.7 parts of sodium hydroxide, 32 parts of water, and 5 parts of sodium sulfate solution. First, the industrial granulated blast furnace slag and the semi-hydrated phosphogypsum are uniformly stirred and mixed in proportion to obtain an inorganic powder mixture. Solid sodium silicate and sodium hydroxide are poured into water in proportion and stirred in a magnetic stirrer to obtain a uniform alkali activator solution. The uniformly stirred alkali activating solution is added to the inorganic powder mixture, and the high-strength semi-hydrated phosphogypsum cementitious material is obtained after uniform stirring. After demolding and curing for 28 days, the material is immersed in a sulfate solution for 28 days and 56 days, and then a mechanical strength test is performed.
[0054]
[0055] Combined with the above data, it can be seen that the present invention obtains a semi-hydrated phosphogypsum-based cementitious material with high residual strength after immersion in sulfate solution for 28 days and 56 days. It can be applied to coastal and salt-immersed land areas to replace cement clinker, and provides a new preparation method for large-scale consumption of phosphogypsum.
[0056] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A method for improving the compressive strength of hemihydrate phosphogypsum cementitious material, characterized in that: After being formed, the phosphogypsum cementitious material is cured with a sulfate ion-containing solution to improve its compressive strength.
2. The method for improving the compressive strength of hemihydrate phosphogypsum cementitious material according to claim 1, characterized in that: The phosphogypsum cementitious material is soaked in a sulfate ion-containing solution after being formed.
3. A high-strength hemihydrate phosphogypsum cementitious material with a large dosage, characterized by: The raw materials include 70-90 parts of hemihydrate phosphogypsum, 10-30 parts of industrial granulated blast furnace slag, 30-40 parts of alkali activator and 2-10 parts of sulfate ion solution by weight.
4. The high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 3 is characterized in that: The sulfate ion-containing solution is a sulfate solution.
5. The high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 4 is characterized in that: The sulfate ion-containing solution is a 5% by mass sodium sulfate solution.
6. The high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 3 is characterized in that: The semi-hydrated phosphogypsum is prepared by calcining phosphogypsum at high temperature.
7. The high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 3 is characterized by: The alkaline activator comprises water glass, sodium hydroxide and water, wherein the water glass comprises 0.3-0.5 parts and the sodium hydroxide comprises 0.5-0.8 parts by weight.
8. The method for preparing a high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 3, characterized in that: The following steps are involved: The semi-hydrated phosphogypsum-based cementitious material prepared from semi-hydrated phosphogypsum, industrial granulated blast furnace slag and an alkali activator is soaked in a sulfate ion-containing solution after being formed.
9. The method for preparing a high-strength hemihydrate phosphogypsum cementitious material with a large dosage according to claim 8, characterized in that: The following steps are involved: (1) uniformly stirring and mixing an alkali activator, hemihydrate phosphogypsum and industrial granulated blast furnace slag to prepare a cementitious material; (2) After the cementitious material has been cured and formed, it is immersed in a solution containing sulfate ions.