Sodium polyacrylate modified asphalt mixture and preparation method thereof

By adding sodium polyacrylate to the asphalt mixture, a highly absorbent hydrogel is formed, which solves the crack filling and permeation problems of asphalt pavement in the frozen soil area, improves the crack resistance and permeability of the pavement, and extends the use of the pavement life.

CN118930133APending Publication Date: 2024-11-12JILIN JIANZHU UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411077825.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Asphalt pavement is prone to early damage in seasonal frozen soil areas with changing climates due to rainwater erosion and low temperature freezing damage, resulting in loose pavement structure, crack formation and moisture penetration, which in turn damages the integrity and stability of the pavement.

Method used

Using sodium polyacrylate (PAAS) modified asphalt mixture, by controlling the content of PAAS in the asphalt mixture, improving water stability and imparting the functions of crack filling and permeation blocking on the road surface. PAAS has high water absorption and plasticity, forming amorphous Hydrogels to fill cracks and prevent moisture from penetration.

Benefits of technology

It significantly improves the low-temperature crack resistance, high-temperature stability and permeability of asphalt mixture, extends the service life of the pavement, prevents moisture erosion and maintains the integrity of the pavement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930133A_ABST
    Figure CN118930133A_ABST
Patent Text Reader

Abstract

The invention provides a sodium polyacrylate modified asphalt mixture and a preparation method thereof, and belongs to the technical field of preparation of highway pavement materials. The sodium polyacrylate modified asphalt mixture comprises the following raw materials: sodium polyacrylate, asphalt, coarse aggregate, fine aggregate and mineral powder, wherein the doping amount of the sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 2%. Sodium polyacrylate has extremely high water absorption and can rapidly absorb water in cracks and expand when micro cracks appear on a pavement, so that the cracks are filled to form soft and amorphous hydrogel, water flow in the cracks or the cracks is effectively inhibited, the water is prevented from further corroding the pavement structure, and the water stability of the asphalt mixture is remarkably improved; and the asphalt pavement is endowed with crack filling and permeation blocking functions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of preparation of highway pavement materials, and in particular relates to a sodium polyacrylate modified asphalt mixture and a preparation method thereof. Background Art

[0002] In seasonally frozen areas with changeable climates, asphalt pavements are often eroded by rainwater and damaged by low temperatures and freezing. Under the combined effect of these factors, the pavement often suffers early damage. Frequent rainfall will weaken the compactness of the asphalt pavement, causing the internal structure of the pavement to become loose, which in turn accelerates the loss of fine particles and destroys the integrity of the pavement. With the arrival of winter, the temperature drops, and the water inside the pavement freezes to produce frost heave force, gradually forming tiny cracks. These cracks become channels for water to invade, further eroding the internal structure of the pavement. If not repaired in time, the asphalt surface layer will cause the asphalt film to peel off from the aggregate surface under the repeated action of pore water pressure, and the aggregates in the mixture will lose their bonding force and gradually soften until they become loose, resulting in roughness and looseness; in local loose areas, the loose aggregate particles gradually fall off and lose, forming potholes of varying sizes. Seepage channels will also form inside the pavement structure, and water will penetrate into the roadbed structure along the seepage path, causing the base layer to deteriorate and destroying the stability of the entire structure.

[0003] Polyacrylate sodium (PAAS), a highly absorbent resin, is a functional polymer material with hydrophilic groups such as hydroxyl and carboxyl groups and a cross-linked network structure. This material has excellent water absorption properties due to its unique three-dimensional network structure. It can quickly absorb and retain water equivalent to hundreds of times its own weight. It still has good water retention at room temperature and is not easy to lose water even under pressure. Compared with other synthetic highly absorbent resins, PAAS has the advantages of better water retention, non-toxicity and environmental protection. Due to its excellent water absorption capacity and compressive resistance, PAAS has been widely used in agriculture, medicine, gardening and construction. When PAAS absorbs water, it forms a PAAS hydrogel with certain viscosity, absorption and plasticity. This hydrogel is amorphous and can gradually release water under certain ion concentrations and pressures. Therefore, in cement concrete, PAAS is often used as an internal curing admixture to improve the performance of cement-based materials; in soil, it is also widely used in water-retaining materials.

[0004] Although PAAS is widely developed and applied in cement-based materials and soil, the application of PAAS in asphalt materials is not enough at present. Therefore, the present invention proposes a sodium polyacrylate modified asphalt mixture and a preparation method thereof. Summary of the invention

[0005] In order to solve the above technical problems, the present invention proposes a sodium polyacrylate modified asphalt mixture and a preparation method thereof, which significantly improves the water stability of the asphalt mixture and imparts the functions of crack filling and penetration blocking to the asphalt pavement by controlling the content of sodium polyacrylate (PAAS) in the asphalt mixture.

[0006] To achieve the above object, the present invention provides a sodium polyacrylate modified asphalt mixture, the raw materials of which include sodium polyacrylate, asphalt and mineral material, and the amount of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 2%;

[0007] The mineral material comprises, by mass percentage, 47% of coarse aggregate, 47% of fine aggregate and 6% of mineral powder.

[0008] Preferably, the oil-to-stone ratio of the sodium polyacrylate modified asphalt mixture is 5%, where the oil-to-stone ratio refers to the percentage of the mass ratio of asphalt to mineral material.

[0009] Preferably, the density of the sodium polyacrylate is less than 200 g / cm 3 , water absorption rate ≥100mL / g, pH value is 6-8, and loss on ignition is 8.09%.

[0010] Preferably, the mineral powder is limestone mineral powder with a particle size less than 0.075 mm.

[0011] Preferably, the grading of the coarse aggregate, fine aggregate and mineral powder is AC-13.

[0012] The present invention also provides a method for preparing the sodium polyacrylate modified asphalt mixture, comprising the following steps:

[0013] The coarse aggregate and the fine aggregate are mixed with asphalt, and then sodium polyacrylate is added and stirred. After the stirring stops, mineral powder is added and the stirring is continued. After the stirring is completed, a sodium polyacrylate modified asphalt mixture is obtained.

[0014] Preferably, the stirring temperature is 160° C. to 165° C., sodium polyacrylate is added and stirred for 1 to 1.5 minutes, and mineral powder is added and stirred for 1.5 to 2 minutes.

[0015] Preferably, the asphalt needs to be heated to 170±5°C before mixing.

[0016] It is a common phenomenon that asphalt pavement has tiny cracks under the influence of traffic loads and environmental factors. The existence of these cracks provides a channel for rainwater to penetrate. Once rainwater enters the cracks, it will form repeated hydrodynamic pressure under the action of traffic loads. This pressure not only exacerbates the expansion of cracks, but also may cause water erosion, thereby further damaging the pavement structure. However, sodium polyacrylate (PAAS) added to asphalt mixtures can significantly improve this situation. PAAS has extremely high water absorption. When microcracks appear on the pavement, PAAS will quickly absorb water in the cracks and expand, thereby filling the cracks and preventing further water penetration. After PAAS absorbs water, it forms a soft and amorphous hydrogel. This hydrogel has good plasticity and will not generate additional internal force on the asphalt mixture under natural conditions. It can effectively inhibit the flow of water in cracks or cracks and prevent water from further eroding the pavement structure. PAAS can not only block the migration of water in the material under water pressure, but also inhibit the penetration of rainwater on the asphalt pavement. In addition, due to the good cyclic water absorption and release capacity of PAAS, as well as the concentration difference between the hydrogel and the atmosphere, the water will be gradually released after a period of time, and the PAAS hydrogel will slowly return to a wet and dry granular material. This property enables PAAS to continuously absorb and release water, thereby maintaining its barrier effect on water during long-term use and improving the anti-permeability performance of asphalt pavement.

[0017] Compared with the prior art, the present invention has the following advantages and technical effects:

[0018] (1) The amount of sodium polyacrylate added in the asphalt mixture of the present invention is 2%. By controlling the amount of sodium polyacrylate added, the asphalt mixture has excellent low-temperature crack resistance, high-temperature stability, water immersion stability and impermeability, and gives the asphalt pavement the function of crack filling and penetration blocking.

[0019] (2) The raw materials of the asphalt mixture of the present invention only include sodium polyacrylate, asphalt and stone, which is environmentally friendly and non-toxic. When the asphalt mixture is mixed and heated, there is no odor or thick smoke. It is physically adsorbed with asphalt and does not change the properties of asphalt. It is cost-effective. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0021] Figure 1 This is a photo of the high temperature and heavy load rutting tester;

[0022] Figure 2 Photo of the Marshall tester;

[0023] Figure 3is the relationship between the dosage of PAAS and the residual stability;

[0024] Figure 4 This is a photo of the electric servo roadbed and pavement material strength testing machine;

[0025] Figure 5 This is the relationship between the dosage of PAAS and the freeze-thaw splitting test strength ratio;

[0026] Figure 6 This is the relationship between PAAS dosage and aggregate loss mass;

[0027] Figure 7 For the schematic diagram of the variable head permeameter structure, see Figure 7 , where 1 is a measuring cylinder, 2 is a valve, 3 is a rubber seal, 4 is a top cover, 5 is a bottom cover, 6 is a valve, 7 is an un-demolded Marshall specimen, 8 is a water inlet pipe, and 9 is a water tank;

[0028] Figure 8 This is a photo of the low temperature crack resistance testing machine;

[0029] Fig. 9 This is the relationship diagram between asphalt mixture with different PAAS content and failure tensile strain;

[0030] Fig.10 This is the relationship between asphalt mixture with different PAAS content and the failure stiffness modulus;

[0031] Fig.11 This is a photo of the high temperature and heavy load rutting tester;

[0032] Fig.12 This is the relationship diagram between the PAAS dosage and the dynamic stability of asphalt mixture. DETAILED DESCRIPTION

[0033] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0034] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0035] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0036] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present invention description and examples are exemplary only.

[0037] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0038] The embodiment of the present invention provides a sodium polyacrylate modified asphalt mixture, the raw materials of which include sodium polyacrylate, asphalt and mineral material, and the amount of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 2%;

[0039] The mineral material comprises, by mass percentage, 47% of coarse aggregate, 47% of fine aggregate and 6% of mineral powder.

[0040] In a preferred embodiment of the present invention, the oil-to-stone ratio of the sodium polyacrylate modified asphalt mixture is 5%, and the oil-to-stone ratio refers to the percentage of the mass ratio of asphalt to mineral material.

[0041] In a preferred embodiment of the present invention, the density of the sodium polyacrylate is less than 200 g / cm 3 , water absorption rate ≥100mL / g, pH value is 6-8, and loss on ignition is 8.09%.

[0042] In a preferred embodiment of the present invention, the mineral powder is limestone mineral powder with a particle size less than 0.075 mm.

[0043] In a preferred embodiment of the present invention, the gradation of the coarse aggregate, fine aggregate and mineral powder is AC-13.

[0044] The embodiment of the present invention also provides a method for preparing the sodium polyacrylate modified asphalt mixture, comprising the following steps:

[0045] The coarse aggregate and the fine aggregate are mixed with asphalt, and then sodium polyacrylate is added and stirred. After the stirring stops, mineral powder is added and the stirring is continued. After the stirring is completed, a sodium polyacrylate modified asphalt mixture is obtained.

[0046] In a preferred embodiment of the present invention, the stirring temperature is 160° C. to 165° C., sodium polyacrylate is added and stirred for 1 to 1.5 minutes, and mineral powder is added and stirred for 1.5 to 2 minutes.

[0047] In a preferred embodiment of the present invention, the asphalt needs to be heated to 170±5°C before mixing.

[0048] The asphalt used in the embodiment of the present invention is AH90# heavy traffic petroleum asphalt. According to the "Test Procedure for Asphalt and Asphalt Mixtures for Highway Engineering" (JTGE20-2011), the penetration of the asphalt is 9 mm, the softening point is 47°C, the elongation is 19.3 cm, the flash point is 280°C, the residual penetration is 65%, and the density is 1.033 g / cm 3 , wax content is 1.7%, and dynamic viscosity is 256Pa·s.

[0049] The ore used in the embodiment of the present invention is composed of coarse aggregate, fine aggregate and mineral powder, wherein the mineral powder is a finely ground ore powder of limestone alkaline material with a particle size of less than 0.075 mm, and the designed gradation of the aggregate is AC-13, which is composed of 1# material (particle size of 9.5-13.2 mm), 2# material (particle size of 4.75-9.5 mm), and 3# material (particle size of 2.36-4.75 mm). The synthetic gradation and gradation curve of AC-13 are shown in Tables 1 and Figure 1 .

[0050] Table 1 Grading composition of mineral materials

[0051]

[0052] The density of the sodium polyacrylate (PAAS) used in the embodiment of the present invention is less than 200 g / cm 3 , water absorption rate ≥100mL / g, pH value 6-8, ignition loss 8.09%. PAAS contains a large number of hydrophilic groups such as carboxyl (-COOH) and hydroxyl (OH), which can form hydrogen bonds with external water molecules to absorb a large amount of free water, thus making PAAS have excellent high water absorption rate, cyclic water absorption capacity and thermal stability.

[0053] In order to meet the requirements of different performance tests, the embodiment of the present invention adopts two methods, compaction molding and wheel rolling molding, to prepare asphalt mixture specimens. Both compaction molding and wheel rolling molding are conventional methods in the field.

[0054] The technical solution of the present invention is further illustrated by the following embodiments.

[0055] Example 1

[0056] (1) Raw material pretreatment

[0057] Dry the coarse aggregate and fine aggregate in an oven at 105°C for 4-6 hours, then place them in an oven and heat them to 180°C;

[0058] Dry PAAS at 60±5℃ for ≥6h;

[0059] Heat the asphalt to 170±5℃;

[0060] Heat the mineral powder to 180°C;

[0061] Weigh the raw materials according to the following weight ratio: the oil-stone ratio is 5%, the amount of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 2%, and the mineral materials are calculated by mass percentage, including 47% coarse aggregate, 47% fine aggregate and 6% mineral powder;

[0062] (2) Preparation method of sodium polyacrylate modified asphalt mixture

[0063] Mix the dried coarse aggregate and fine aggregate with the preheated asphalt, then add PAAS and stir in a mixer for 1 to 1.5 minutes. After the stirring stops, add the heated mineral powder and continue stirring for 1.5 to 2 minutes to ensure that all ingredients are evenly mixed. During the entire mixing process, the temperature needs to be maintained between 160°C and 165°C. After the mixing is completed, a sodium polyacrylate modified asphalt mixture (2% PAAS asphalt mixture) is obtained.

[0064] Comparative Example 1

[0065] The same as Example 1, except that the dosage of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 4%, and a PAAS asphalt mixture with a dosage of 4% is obtained.

[0066] Comparative Example 2

[0067] The same as Example 1, the only difference is that the dosage of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 6%, and a PAAS asphalt mixture with a dosage of 6% is obtained.

[0068] Comparative Example 3

[0069] The same as Example 1, the only difference is that the dosage of sodium polyacrylate in the sodium polyacrylate modified asphalt mixture is 8%, and the PAAS asphalt mixture with 8% dosage is obtained.

[0070] Comparative Example 4

[0071] The same as Example 1, except that the amount of sodium polyacrylate added to the sodium polyacrylate modified asphalt mixture is 0%, and a common asphalt mixture is obtained.

[0072] The asphalt mixtures obtained in Example 1 and Comparative Examples 1 to 4 were subjected to the following performance tests:

[0073] 1. Immersion Marshall Test

[0074] Place the prepared asphalt mixture specimens in a constant temperature water bath and cure until the specimens reach sufficient strength. Place the cured specimens in a Marshall tester ( Figure 2 ), adjust the test instrument so that it can accurately apply the load, start the Marshall stability tester, and make the asphalt mixture specimen bear the load. When the Marshall stability tester automatically pauses, read the pressure and flow values ​​displayed on the tester, and calculate the water immersion residual stability according to the following formula:

[0075]

[0076] Where: MS o —Residual stability of the specimen after immersion in water (%); MS1—Stability of the specimen after immersion in water for two days (KN); MS—Marshall stability of the specimen (KN).

[0077] The results of the Marshall test of asphalt mixtures immersed in water of Example 1 and Comparative Examples 1 to 4 are shown in Table 2. The relationship between the dosage of PAAS and the residual stability is shown in Table 2. Figure 3 .

[0078] Table 2 Marshall test results

[0079]

[0080] According to the specification, the stability of asphalt mixture should reach or exceed 80%. Figure 3 It can be seen that the residual stability of asphalt mixtures with different PAAS (sodium polyacrylate) dosages is significantly different. With the increase of PAAS dosage, the stability shows a gradually decreasing trend. Specifically, compared with asphalt mixtures without PAAS, the residual stability of asphalt mixtures with 2%, 4%, 6% and 8% PAAS dosages decreased by 2%, 3%, 3% and 2%, respectively. This shows that the addition of PAAS has a negative impact on the retention stability of asphalt mixtures. The reason for the decrease in the water stability of asphalt mixtures may be that the hydrogel formed by PAAS in the asphalt mixture plays a lubricating role in the interface between aggregates, thereby weakening the close connection between aggregate particles through asphalt mortar, so the addition of PAAS leads to a decrease in the water stability of asphalt mixtures. Although the retention stability of PAAS-modified asphalt mixtures meets the requirements of the specification, the residual stability of water immersion gradually decreases due to the increase in the PAAS dosage, so the PAAS dosage should not exceed 2%.

[0081] 2. Freeze-thaw splitting test

[0082] Place the prepared asphalt mixture specimens in a constant temperature water bath and cure until the specimens reach sufficient strength. Operate the microcomputer-controlled electric servo roadbed and pavement material strength testing machine ( Figure 4 ), and turn on the temperature control box, select the splitting strength test mode on the pavement strength instrument, adjust the fixture for the freeze-thaw splitting test, install the displacement sensor, and perform zeroing. Keep the equipment running, remove the specimen from the water bath at a constant temperature of 25℃±0.5℃, and wipe the surface moisture with a towel. Place the specimen between the upper and lower pressure heads of the splitting fixture, start the instrument, align the loading device with the small groove of the fixture, and start the test. As the chassis rises, load until the specimen is destroyed. The instrument will display the loading displacement graph, displacement peak and maximum load, and automatically stop the motor. Before conducting the next set of tests, clean the debris and moisture on the fixture to avoid affecting the subsequent test results. After ensuring that the test environment is consistent, perform the operation, and pay attention to recording the data of each test and marking it for analysis and summary of the test rules. The splitting tensile strength of the standard Marshall specimen is calculated according to the following formula:

[0083]

[0084] Where: TSR—freeze-thaw splitting test strength ratio (%); RT1—average splitting tensile strength of the first group of specimens without freeze-thaw cycles (MPa); RT2—average splitting tensile strength of the second group of specimens after freeze-thaw cycles (MPa).

[0085] The results of the splitting tensile strength test of asphalt mixtures of Example 1 and Comparative Examples 1 to 4 are shown in Table 3. The relationship between the dosage of PAAS and the freeze-thaw splitting test strength ratio (%) is shown in Table 3. Figure 5 .

[0086] Table 3 Splitting tensile strength test results

[0087]

[0088] From Table 3 and Figure 5 It can be seen that with the addition of PAAS (sodium polyacrylate), PAAS can absorb water inside the asphalt mixture to form a hydrogel. When the temperature drops below 0°C, the water in the hydrogel freezes, causing the volume of the hydrogel in the pores to expand. This expansion will cause expansion stress on the matrix of the asphalt mixture, because the matrix of the asphalt mixture will become harder and more brittle at low temperatures and cannot resist this expansion stress well. Therefore, the repeated freezing and expansion of the hydrogel will cause damage inside the asphalt mixture, and these damages will accumulate with the number of freeze-thaw cycles. With the increase in the PAAS dosage, the amount of hydrogel in the mixture will also increase, so the expansion stress generated during the freeze-thaw cycle will also increase. This expansion stress will cause greater damage to the internal structure of the asphalt mixture, resulting in a decrease in the splitting tensile strength of the asphalt mixture.

[0089] 3. Fort Kentucky Dispersion Test

[0090] Install the cured specimens on the Kentenberg scattering tester, and adjust the loading device to ensure that it can accurately apply the load. After starting the test machine, record the number of scattered particles and particle size distribution of the specimen under load. When the number of scattered particles of the specimen reaches the specified standard, stop the test and record the number of specimen losses. By analyzing the test data, the anti-scattering performance of asphalt mixtures in a dry environment can be evaluated. Each group of specimens has 4 parallel samples. Example 1, Comparative Examples 1 to 4 The Kentenberg scattering test results of asphalt mixtures are shown in Table 4, and the relationship between PAAS dosage and aggregate loss mass is shown in Figure 6 .

[0091] Table 4 Kentucky Fort dispersion test results

[0092]

[0093] From Table 4 and Figure 6 It can be seen that the weight loss tested in the Kentucky Fort test continues to increase with the increase of PAAS content, but all meet the specification requirement of less than 20%. In addition, the mass loss of aggregate under the soaked condition is significantly greater than that under the unsoaked condition, and the growth rate of the mass loss is significantly accelerated with the increase of PAAS content. This is because after immersion in the water bath for 20 hours, PAAS absorbs water to form hydrogels in the asphalt mixture and fills the pores in the asphalt mixture. When the asphalt mixture is subjected to impact or load, these hydrogels will deform together with the asphalt matrix. However, due to the low elastic modulus of hydrogels, they are more likely to deform and break when subjected to external forces. This leads to a decrease in the bonding force between the hydrogel and the asphalt matrix, weakens the adhesion between the asphalt and the aggregate, and makes the aggregate more likely to fall off during the collision. In addition, in the Kentucky Fort scattering test, the internal PAAS also plays a lubricating role in the mixture, and the friction between the aggregates is reduced, making them more likely to slide relative to each other during the collision, resulting in more aggregate falling off. Therefore, the weight loss caused by the Kentucky Fort dispersion test continued to increase with the increase of PAAS content.

[0094] 4. Permeability test

[0095] The permeability test was conducted based on porous media theory and Darcy's law to determine the permeability coefficient K. The side wall leakage problem was solved by using a sealing ring and a method of not demoulding the test piece. The schematic diagram of the variable head permeameter is shown in Figure 7 , where 1 is a measuring cylinder, 2 is a valve, 3 is a rubber seal, 4 is a top cover, 5 is a bottom cover, 6 is a valve, 7 is an undemolded Marshall specimen, 8 is a water inlet pipe, and 9 is a water tank.

[0096] Specific operation steps of variable head permeameter:

[0097] (1) Place the rubber sealing ring into the groove of the top cover and press it firmly by hand.

[0098] (2) Place filter paper in the bottom cover to prevent small particles of the asphalt mixture from falling off and clogging the water outlet pipe during the test.

[0099] (3) Place the asphalt concrete specimen between the top cover and the bottom cover and adjust the position to ensure that there is no gap between the specimen and the top cover and the bottom cover.

[0100] (4) Use waterproof tape to fix the top cover and bottom cover to the Marshall mold respectively to prevent water from seeping from the edges and provide double protection.

[0101] (5) After the instrument is connected and aligned, open valve 2 and valve 6, and fill water into the water inlet pipe, using gravity to fully inject water into the instrument. When the water level in the measuring cylinder 1 reaches a certain height, stop filling water, close valve 6, and remove the water inlet pipe 8.

[0102] (6) Open valve 6 and let a small amount of water flow out so that the water can completely fill the entire test piece to reduce errors.

[0103] (7) Record the height of the liquid level in the measuring cylinder at the beginning of the test (t1) (h1) and the height of the liquid level in the measuring cylinder at the end of the test (t2) (h2).

[0104] Before the test begins, use a test piece with extremely small porosity and no water permeability for testing. If the liquid level in the measuring cylinder does not change after 1 hour of testing, it means that the side wall is not leaking and the permeability coefficient of the test piece can be accurately measured. The calculation formula for the variable head permeability coefficient K is as follows:

[0105]

[0106] Where: K—permeability coefficient, mm / s;

[0107] a—Cross-sectional area of ​​penetration specimen, cm 2 ;

[0108] L—average height of penetration specimen, cm;

[0109] A—Internal cross-sectional area of ​​the measuring cylinder, cm 2 ;

[0110] t—total penetration time (t2-t1), s;

[0111] h1—the height of the liquid level in the measuring cylinder at the initial timing, cm;

[0112] h2—the height of the liquid level in the measuring cylinder at the end of the timing, cm;

[0113] The average height L of the penetration test piece was measured to be 63.5 mm, and the cross-sectional area a of the penetration test piece was calculated to be 324 cm 2 The cross-sectional area A of the measuring cylinder is 254 cm 2 .

[0114] The results of the determination of the permeability coefficient K of the asphalt mixtures of Example 1 and Comparative Examples 1 to 4 are shown in Table 5.

[0115] Table 5 Permeability coefficient K measurement results

[0116] Asphalt Type K(mm / s) Ordinary asphalt mixture 0.06296 2% PAAS asphalt mixture 0.04006 4% PAAS asphalt mixture 0.03303 6% PAAS asphalt mixture 0.03167 8% PAAS asphalt mixture 0.02956

[0117] It can be seen from Table 5 that the permeability coefficient of the asphalt mixture modified by PAAS is significantly reduced compared with that of the ordinary asphalt mixture. When the PAAS content is 2%, 4%, 6%, and 8%, the permeability coefficient is reduced by 36.37%, 47.61%, 49.84%, and 53.04%, respectively. This shows that the more PAAS is added to the asphalt mixture, the more significant the effect of PAAS on reducing water penetration.

[0118] 5. Low temperature splitting test

[0119] Place the compacted Marshall specimens in a low-temperature environment box and set the temperature in the box to -10°C. Ensure that there is an appropriate space between each specimen (usually not less than 10mm) and keep them in the box for more than 6 hours to meet the requirements of the low-temperature splitting test. At the beginning of the test, start the low-temperature cracking test machine ( Figure 8 ) and select the split test mode, take out the asphalt mixture specimen from the environmental chamber and place it in the split test fixture, making sure that the specimen is in the center of the fixture and the upper and lower parts of the fixture are aligned with the crosshairs marked on the specimen.

[0120] After the fixture position is adjusted properly, the displacement sensor is installed to ensure that it can accurately capture the impact of the upper and lower loading, and is calibrated and zeroed. Next, the loading column is pre-pressed to a position close to the groove but not yet in contact, in preparation for the low-temperature splitting test.

[0121] Connect the pavement strength tester to the temperature control box and loading device properly, and adjust the loading rate to an appropriate level. The deformation caused by the downward pressure of the pressure head is in the vertical direction of the specimen, and the loading rate is 50mm / min. During the experiment, the screen of the tester will display the curve of the loading displacement.

[0122] After the test is started, the loading column begins to press down, and the low-temperature splitting fixture is stressed and contacts the specimen. The test continues until the specimen breaks, at which point the test ends automatically. The test machine displays the peak deformation and maximum failure load values, which need to be recorded, saved, and backed up for subsequent test result analysis.

[0123] The results of the low temperature crack resistance test of asphalt mixtures of Example 1 and Comparative Examples 1 to 4 are shown in Table 6.

[0124] Table 6 Low temperature crack resistance test results

[0125]

[0126] The relationship between asphalt mixture with different PAAS content and tensile strain at failure and stiffness modulus at failure is shown in Fig. 9 and Fig.10 ,Depend on Fig. 9 and Fig.10 As shown in Table 6, at a dosage of 2%, the asphalt mixture has the smallest failure stiffness modulus and the largest failure tensile strain, which means that the PAAS asphalt mixture has the best low-temperature crack resistance of asphalt at this time. This is because the appropriate amount of PAAS absorbs water and PAAS can fill the voids in the asphalt mixture, reduce the void ratio, and thus improve the density and strength of the mixture. The shrinkage and deformation of the asphalt mixture will be reduced at low temperatures, which will improve the low-temperature crack resistance of the asphalt mixture. Thereafter, as the dosage of PAAS increases, excessive addition of PAAS may cause uneven distribution of particles in the mixture and reduce the bonding force between asphalt and PAAS particles. In addition, excessive addition of PAAS may affect the density of the asphalt mixture, aggravate the shrinkage and deformation of the mixture at low temperatures, thereby increasing the formation of cracks, and during the freeze-thaw cycle, the gel formed by excessive PAAS particles may expand and shrink when the temperature changes, resulting in damage accumulation inside the asphalt mixture and reducing the crack resistance of the mixture.

[0127] 6. Stability test

[0128] The Marshall stability (MS) of the asphalt mixtures of Example 1 and Comparative Examples 1 to 4 was measured according to the method in JTG E20-2011. The results are shown in Table 7.

[0129] Table 7 Marshall stability test results

[0130] Asphalt mixture type MS(KN) Ordinary asphalt mixture 10.35 2% PAAS asphalt mixture 10.72 4% PAAS asphalt mixture 10.11 6% PAAS asphalt mixture 9.57 8% PAAS asphalt mixture 8.91

[0131] As can be seen from Table 7, it can be seen that asphalt mixtures with different PAAS (sodium polyacrylate) contents can meet the requirements of not less than 8KN in the specification in terms of Marshall stability. When the PAAS content is 2%, due to the small particle size of PAAS, it can be more closely combined with asphalt, thereby improving the overall stability of the mixture. This is because PAAS particles can more fully fill the voids in the asphalt mixture and enhance the bonding force between asphalt and aggregate. However, with the increase of PAAS content, the content exceeding 2% may cause the distribution of PAAS particles in the asphalt mixture to become uneven, which will cause the voids between PAAS particles to increase, resulting in a decrease in the bonding between PAAS and asphalt, thereby affecting its high temperature stability.

[0132] 7. High temperature rutting test

[0133] The dynamic stability (DS) of the asphalt mixtures of Example 1 and Comparative Examples 1 to 4 at 60°C was measured according to the method in JTG E20-2011. The photo of the high temperature and heavy load rutting tester is shown in Fig.11 The test results are shown in Table 8. The relationship between the dosage of PAAS and the dynamic stability of asphalt mixture is shown in Fig.12 .

[0134] Table 8 Dynamic stability (DS) at 60°C

[0135] Asphalt mixture type Dynamic stability (DS) Ordinary asphalt mixture 1322 2% PAAS asphalt mixture 1379 4% PAAS asphalt mixture 1320 6% PAAS asphalt mixture 1283 8% PAAS asphalt mixture 1254

[0136] From Table 8 and Fig.12 It can be seen that the dynamic stability test results of PAAS asphalt mixture can be observed. The dynamic stability of all PAAS-modified asphalt mixtures exceeded 1000 times / mm, which meets the requirements of the specification, indicating that these asphalt mixtures have strong deformation resistance under dynamic loading. Secondly, with the increase of PAAS content, the dynamic stability of the asphalt mixture shows a trend of first rising and then falling. When the PAAS content is 2%, the dynamic stability reaches the highest 1379 times / mm; with the increase of the content, the dynamic stability gradually decreases, and when the PAAS content is 8%, the dynamic stability is 1254 times / mm. This trend is consistent with the results of the Marshall stability test, that is, the addition of excessive PAAS leads to a decrease in the stability of the asphalt mixture. This phenomenon is because with the increase of PAAS content, the number of PAAS particles in the asphalt mixture increases, resulting in a decrease in the density of the asphalt mixture, thereby affecting the deformation resistance of the asphalt mixture. In addition, the increase of PAAS particles may affect the bonding between asphalt and aggregate, thereby affecting the dynamic stability of the asphalt mixture.

[0137] In summary, the present invention sets the dosage of sodium polyacrylate in the asphalt mixture to 2%, so that the asphalt mixture has excellent low-temperature crack resistance, high-temperature stability, water immersion stability and impermeability.

[0138] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A sodium polyacrylate modified asphalt mixture, characterized in that: The raw materials include sodium polyacrylate, asphalt and mineral material, wherein the sodium polyacrylate is added in an amount of 2% in the sodium polyacrylate modified asphalt mixture; The mineral material comprises, by mass percentage, 47% of coarse aggregate, 47% of fine aggregate and 6% of mineral powder.

2. The sodium polyacrylate modified asphalt mixture according to claim 1, characterized in that: The oil-stone ratio of the sodium polyacrylate modified asphalt mixture is 5%.

3. The sodium polyacrylate modified asphalt mixture according to claim 1, characterized in that: The density of the sodium polyacrylate is less than 200 g / cm 3 , water absorption rate ≥100mL / g, pH value is 6-8, and loss on ignition is 8.09%.

4. The sodium polyacrylate modified asphalt mixture according to claim 1, characterized in that: The mineral powder is limestone mineral powder with a particle size less than 0.075 mm.

5. The sodium polyacrylate modified asphalt mixture according to claim 1, characterized in that: The gradation of the coarse aggregate, fine aggregate and mineral powder is AC-13.

6. A method for preparing a sodium polyacrylate modified asphalt mixture according to any one of claims 1 to 5, characterized in that: The following steps are involved: The coarse aggregate and the fine aggregate are mixed with asphalt, and then sodium polyacrylate is added and stirred. After the stirring stops, mineral powder is added and the stirring is continued. After the stirring is completed, a sodium polyacrylate modified asphalt mixture is obtained.

7. The method for preparing the sodium polyacrylate modified asphalt mixture according to claim 6, characterized in that: The stirring temperature is 160° C. to 165° C., sodium polyacrylate is added and stirred for 1 to 1.5 minutes, and mineral powder is added and stirred for 1.5 to 2 minutes.

8. The method for preparing sodium polyacrylate modified asphalt mixture according to claim 6, characterized in that: The asphalt is heated to 170±5°C before mixing.