Geopolymer grouting material for rapid recovery of bearing capacity of semi-flexible pavement as well as preparation method and fixed-point repairing process of geopolymer grouting material
By preparing and applying geopolymer grouting materials, combined with targeted repair techniques, the problems of high energy consumption, significant resource waste, and insufficient adhesion of semi-flexible pavement grouting materials have been solved, achieving efficient and low-cost pavement load-bearing capacity restoration and environmentally friendly construction.
Patent Information
- Application Number
- CN202410903018.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing semi-flexible pavement grouting materials suffer from high energy consumption, significant resource waste, complex construction, and high material costs during production. Furthermore, the adhesion and stability between the grouting material and the parent asphalt mixture are insufficient, resulting in low pavement load-bearing capacity recovery efficiency.
A new type of grouting material is prepared by using geopolymer grout, water-reducing agent, shrinkage-reducing agent, sand and powder, combined with alkali activator. This material improves the drying shrinkage rate and fluidity. It is also used for efficient penetration grouting through a targeted repair process to ensure that the grouting material accurately penetrates into the defective areas of the base layer.
It improves the high-temperature and water stability of semi-flexible pavements, reduces energy consumption and material costs, achieves rapid load-bearing capacity recovery, reduces construction time and environmental pollution, and meets safety and environmental protection requirements.
Smart Images

Figure CN118930137A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of road engineering, and in particular relates to a geopolymer grouting material for rapid recovery of semi-flexible road bearing capacity, a preparation method thereof, and a grouting material fixed-point repairing process. Background Art
[0002] Semi-flexible pavement is a new type of pavement composed of asphalt mixture and cement-based grouting materials. It has the advantages of both asphalt pavement and cement pavement, and is a rigid and flexible pavement structure. However, the cement slurry poured into the semi-flexible pavement will produce a large amount of waste gas emissions such as CO2 and SO2 during its production process, and will cause a large amount of energy consumption and resource waste. A series of grouting materials such as ordinary silicates, volcanic ash modified concrete, and fiber-modified cement-based materials have been developed at home and abroad. Most of them are cement-based materials, which have defects such as high energy consumption and high cost, and some materials have complex construction processes. Therefore, it is necessary to consider replacing cement grouting materials in semi-flexible materials. Geopolymer grouting material is an alkali activator gelling material. The raw materials come from industrial wastes such as fly ash, kaolin, and slag. Such raw materials are rich in silicon-aluminum phase raw materials. Under the action of alkali activators, the addition of admixtures makes the reaction rate of silicate faster and the reaction product higher. At the same time, the polymerization reaction generates a three-dimensional network gel. Compared with ordinary cement mortar, geopolymer grouting material has the advantages of high compressive strength, good durability and corrosion resistance, early strength and fast hardening. Combined with relevant construction technology, it can make the grouting material firmly bonded with the parent asphalt mixture, making the internal pavement structure more dense, quickly improving the bearing capacity of the semi-flexible pavement and extending the service life of the road. And because the raw materials are taken from industrial waste, geopolymer grouting materials are abundant and low in price, so the actual use requires little energy consumption and causes less pollutant emissions. Summary of the invention
[0003] Purpose of the invention: The purpose of the present invention is to provide a polymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement, and a preparation method and a fixed-point repair process thereof. The grouting material has performance advantages such as resistance to rutting, high temperature resistance, good adhesion and excellent low-temperature stability, and economic advantages of reasonable design, saving consumables and saving costs; Another purpose of the present invention is to provide a preparation method for a polymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement. The method is simple in process, green and low-carbon, conducive to industrial production, and the main raw materials are environmentally friendly, and the specific construction and use are convenient; Another purpose of the present invention is to provide a fixed-point repair process for a polymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement. Combined with the prepared grouting material, the construction process is adopted to improve the construction efficiency while ensuring the construction quality, improve the bearing capacity of the semi-flexible pavement, and meet the requirements of safety and environmental protection.
[0004] Technical solution: The present invention discloses a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement, a preparation method thereof and a fixed-point repair process. The geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement comprises an aqueous polyurethane emulsion, a water reducer, a shrinkage reducer, sand, powder and an alkali activator; wherein, based on the raw materials of the geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement, in parts by weight, the aqueous polyurethane emulsion is 1 to 3 parts, the water reducer is 1 to 3 parts, the shrinkage reducer is 1 to 3 parts, the sand is 10 to 30 parts, the powder is 95 to 105 parts and the alkali activator is 65 to 70 parts; the aqueous polyurethane emulsion added to the geopolymer has a synergistic viscosity-increasing and stabilizing effect, effectively improving the shrinkage rate of the geopolymer, the added water reducer can effectively improve the fluidity and strength of the geopolymer, and the added shrinkage reducer can effectively offset the shrinkage that may occur during the hardening process of the geopolymer. The invention improves the high temperature stability and water stability of the existing common semi-flexible pavement grouting material, making it suitable for grouting in various important road sections or areas requiring high strength and rutting resistance.
[0005] Preferably, the aqueous polyurethane emulsion has a molecular weight of 5000-10000 and a solid content of 30%. Improve the shrinkage of geopolymers.
[0006] Preferably, the water reducer is a high-concentration naphthalene-based water reducer, which has the characteristics of high water reduction rate, high reinforcement and no air entrainment.
[0007] Preferably, the shrinkage reducing agent is a polycarboxylic acid high-efficiency shrinkage reducing agent, which mainly functions to offset the shrinkage that may occur during the hardening process of the geopolymer and increase the strength of the geopolymer.
[0008] Preferably, the fly ash has a specific surface area of 0.314 m 2 / g, the specific surface area of blast furnace slag is 0.428m 2 / g.
[0009] Preferably, the alkaline activator is a mixture of solid sodium hydroxide and water glass, wherein the solid sodium hydroxide is flaky solid particles with a purity of 99%, the molecular formula of the water glass is Na2O·3.3SiO2, and the modulus of the water glass is 2.0-2.5.
[0010] The method for preparing a geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity of the present invention comprises the following steps: (1) 57-63 parts of fly ash and 38-42 parts of blast furnace slag are uniformly dry-mixed for 30 seconds to obtain a powder; (2) Weigh 10-30 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 43-48 parts of water; (3) Preparation of alkali activator: Add sodium hydroxide and water glass to water and stir evenly to prepare an alkali activator with an alkali equivalent of 4% to 7% and a water glass modulus of 2.0 to 2.5, and let it stand for 24 hours; (4) Add 1-3 parts of waterborne polyurethane emulsion, 1-3 parts of water reducing agent, 1-3 parts of shrinkage reducing agent, 65-70 parts of alkali activator and the remaining water to 95-105 parts of powder, rotate at 100-150 r / min, and slowly stir for 120 seconds to obtain a gel material; (5) Finally, the rotation speed is 250-300 r / min, and the cementitious material is quickly stirred for 120 s to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0011] The fixed-point repair process of the geopolymer grouting material for rapid recovery of the bearing capacity of the semi-flexible pavement of the present invention comprises the following steps: (1) Material selection, mix optimization and grouting material preparation; (2) Construction process: The semi-rigid base layer is thoroughly cleaned to remove loose materials and impurities to ensure that the grouting area is clean and dry. According to the pavement conditions and the deflection basin index (BDI) analysis results, the drilling position and spacing are reasonably arranged using fixed-point technology to ensure that the grouting material can penetrate into the defective area of the base layer more accurately and reduce interference with the surrounding intact structures. The static pressure method is used for polymer fixed-point penetration grouting. By reducing the number of compaction times to simulate the condition of insufficient density, the bearing capacity is tested, and the feasibility of polymer penetration grouting is analyzed. The pressure is controlled not to exceed 0.3 MPa during the grouting process.
[0012] (3) Quality control: real-time monitoring of grouting pressure, grouting volume and grouting depth during construction to ensure construction quality; measurement of pavement deflection and geological radar detection after grouting, and maintenance of the construction area.
[0013] (4) Construction safety management and environmental protection: Strictly abide by safety regulations during the construction process to ensure the safety of construction personnel and equipment; take measures to reduce noise pollution during the construction process and protect the surrounding environment.
[0014] Compared with the prior art, the present invention has the following significant advantages: (1) The geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement is added with water-based polyurethane emulsion. Through the synergistic effect of the water-based polyurethane emulsion and the inorganic substance of blast furnace slag, siloxane is formed, so that two functional groups, namely, organic-philic and inorganic-philic, exist in the molecule, thereby increasing the cohesion of the geopolymer and the asphalt mixture and improving the high-temperature stability of the semi-flexible pavement material; (2) The geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement can be synergistically acted with fly ash. The water-based polyurethane emulsion is condensed together and dehydrated to form a film, which is interwoven with the gel product and the unhydrated powder particles to form a network structure, making the material structure more compact. As the strength of the geopolymer grouting material increases, the water stability of the semi-flexible material is also improved; (3) The water glass modulus of the geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement is preferably 2.0-2.5, and the slurry prepared is The material has the advantages of high mechanical properties, small shrinkage and good fluidity, and is suitable for grouting in various important road sections or areas that require high strength and rutting resistance; (4) The geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity uses fly ash and slag construction waste as raw materials to reduce the raw material cost of the grouting material; compared with conventional cement grouting materials, geopolymer grouting materials have less energy consumption and less waste emissions, achieving green and sustainable development of grouting materials; (5) The fixed-point repair process of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity uses fixed-point technology to reasonably arrange the drilling position and spacing, which can ensure that the grouting material can penetrate into the defective area of the base more accurately and reduce interference with the surrounding intact structures; (6) The fixed-point repair process of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity uses static pressure method for polymer fixed-point penetration grouting. During the grouting process, the pressure is controlled not to exceed 0.3MPa, which can prevent damage to the surrounding structures. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a flow chart of the preparation and construction of the geopolymer grouting material for rapid recovery of the bearing capacity of the semi-flexible pavement according to the present invention; Figure 2 This is a cross-sectional view of a typical base collapse rutting pavement; Figure 3 The invention provides a construction drawing for spot repair of geopolymer grouting material for rapid recovery of the bearing capacity of the semi-flexible pavement.
[0016] Among them, 1-pavement collapse area; 2-surface layer; 3-collapsed base layer; 4-cushion layer; 5-soil base; 6-base collapsed rutting road surface; 7-grouting engineering vehicle; 8-base disease area; 9-fixed-point repair grouting holes. DETAILED DESCRIPTION
[0017] The technical solution of the present invention is further described below in conjunction with specific examples.
[0018] The chemical composition of fly ash in the present invention is shown in Table 1; the chemical composition of blast furnace slag is shown in Table 2; the sand grading is shown in Table 3; the water-based polyurethane emulsion has a solid content of 30% and a viscosity of 1000-1200 CPS, and is a milky white blue liquid produced by Shanghai McLean Biochemical Technology Co., Ltd.; the water reducer is a high naphthalene series water reducer produced by Shandong Liangzheng New Materials Technology Co., Ltd.; the shrinkage reducing agent is a polycarboxylic acid high-efficiency water reducer produced by Jiangsu Subote New Materials Co., Ltd.
[0019] Example 1 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0020] Example 2 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 3 parts of sodium hydroxide, 43 parts of water glass and 17 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.0, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0021] Example 3 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 3.5 parts of sodium hydroxide, 44 parts of water glass and 18 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.5, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0022] Example 4 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 5.5 parts of sodium hydroxide, 22 parts of water glass and 30 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 1.0, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0023] Example 5 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: Mix 1 part of sodium hydroxide, 64 parts of water glass and 4 parts of water, and stir evenly to make an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 3.0, and let it stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0024] Example 6 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; 2 parts of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator are added to 100 parts of powder and slowly stirred for 120 seconds to obtain a gel material; finally, the gelling material is quickly stirred for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0025] Example 7 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 3 parts of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0026] Example 8 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; 0 parts of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator are added to 100 parts of powder and slowly stirred for 120 seconds to obtain a gel material; finally, the gelling material is quickly stirred for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0027] Example 9 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 5 parts of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0028] Example 10 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 30 parts of water; Preparation of alkaline activator: 2 parts of sodium hydroxide, 48 parts of water glass and 2 parts of water are mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0029] Embodiment 11 refer to Figure 1The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 40 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 49 parts of water glass and 8 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0030] Example 12 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 60 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 49 parts of water glass and 28 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 1 part of water reducing agent, 1 part of shrinkage reducing agent, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0031] Example 13 refer to Figure 1 The preparation steps of the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity are as follows: 60 parts of fly ash and 40 parts of blast furnace slag were uniformly dry-mixed for 30 seconds to obtain a powder; Weigh 20 parts of sand, dry mix the powder and sand evenly for 30 seconds, and weigh 45 parts of water; Preparation of alkaline activator: 2.5 parts of sodium hydroxide, 50 parts of water glass and 15 parts of water were mixed evenly to prepare an alkaline activator with an alkali equivalent of 6% and a water glass modulus of 2.3, and then allowed to stand for 24 hours; Add 1 part of water-based polyurethane emulsion with a solid content of 30%, 6 parts of water reducer, 1 part of shrinkage reducer, and 67.5 parts of alkali activator into 100 parts of powder and stir slowly for 120 seconds to obtain a gel material; finally, stir the gelling material quickly for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
[0032] With reference to the specifications T0508, JGJ / T 70 and T0506, the fluidity, shrinkage rate and compressive strength performance of the geopolymer grouting material based on the semi-flexible pavement provided by the present invention were tested. As shown in Table 4.
[0033] Referring to the specification JGJ E20-2011, the geopolymer grouting material based on the semi-flexible pavement provided by the present invention was subjected to a low-temperature small beam bending test of a geopolymer asphalt mixture, as shown in Table 5.
[0034] As shown in Table 4 and Table 5, the geopolymer grouting material prepared in Example 1 has the best performance, good fluidity, and is easy to grout; the shrinkage rate is small, and the adhesion with the parent asphalt mixture is good; the compressive strength increases quickly, and it can quickly bear heavy loads. The optimal ratio of the geopolymer grouting material can be selected as follows: the alkali equivalent of the alkali activator is 6%, the water glass modulus is 2.3, the sand: fly ash: slag: water is 1:3:2:2.25; the water reducer is 1%; the waterborne polyurethane emulsion is 1%; and the shrinkage reducer is 1%.
[0035] The present invention provides a geopolymer grouting material for rapid recovery of bearing capacity of a semi-flexible pavement, to which admixtures such as water-based polyurethane emulsion are creatively added, which synergize with fly ash, and the water-based polyurethane emulsion is condensed and dehydrated to form a film, which is interwoven with gel products and unhydrated powder particles to form a network structure, making the internal structure of the material more dense, and with the continuous increase in the strength of the geopolymer grouting material, the low-temperature crack resistance of the semi-flexible material is improved. The modulus of the water glass in the alkali activator prepared from water glass and sodium hydroxide is 2.0-2.5. When the modulus of the alkali activator is too small, the alkalinity is strong and the coagulation rate is fast, which easily leads to insufficient grouting in the later stage; when the modulus of the alkali activator is too large, the powder cannot be fully activated and the mechanical properties cannot meet the requirements.
[0036] The water-cement ratio of the geopolymer grouting material prepared by the present invention is 0.4-0.5. Since the higher the water-cement ratio, the lower the fluidity of the grouting material, but the 7d compressive strength is also reduced accordingly, it can be seen that although the increase of water can reduce the fluidity, it will have a negative impact on the compressive strength of the geopolymer. Therefore, it is necessary to select an optimal water-cement ratio so that the fluidity and compressive strength of the geopolymer are optimized.
[0037] As shown in Table 5, the high-temperature performance of semi-flexible pavement materials is much higher than that of conventional asphalt pavement materials. This is because the addition of water-based polyurethane emulsion and blast furnace slag inorganic substances synergistically combine to form siloxane. There are two functional groups in the molecule, one is organic-philic and the other is inorganic-philic. This bridges the gap between inorganic and organic materials, increases the bonding strength between materials, increases the cohesion between geopolymers and asphalt mixtures, and improves the low-temperature crack resistance of semi-flexible pavement materials.
[0038] Figure 2 A cross section of a typical pavement showing base collapse and rutting is shown. In this image, the various layers of the pavement can be clearly seen, including the surface layer 2, base layer 3, cushion layer 4, and subgrade 5. The collapsed area 1 of the pavement is usually caused by damage or loss of the base material. This collapse can cause uneven settlement of the pavement, which in turn causes rutting.
[0039] Figure 3 The construction process of using the geopolymer grouting material of the present invention for fixed-point repair is described in detail. The figure shows the operation of the grouting engineering vehicle 7 to carry out fixed-point repair grouting holes 9 in the base defect area 8. The arrangement of the grouting holes is determined based on the road surface conditions and the deflection basin index (BDI) analysis results to ensure that the grouting material can effectively penetrate into the defective area of the base.
[0040] In the construction process of the geopolymer grouting material fixed-point repair process for the rapid recovery of the bearing capacity of a semi-flexible pavement provided by the present invention, the semi-rigid base is firstly cleaned thoroughly to remove loose materials and impurities to ensure that the grouting area is clean and dry. Figure 2 Subgrade collapse and rutting conditions in Figure 3 The construction process shown in the figure is to arrange the position and spacing of the grouting holes reasonably. The static pressure method is used for grouting, and the grouting pressure is controlled not to exceed 0.3MPa to prevent damage to the surrounding structure. After the grouting is completed, the pavement deflection value is measured and the geological radar is detected to ensure the construction quality. Finally, the construction area is maintained to ensure that the repaired pavement has the required bearing capacity and stability.
[0041] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention may be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the claims of the present invention.
[0042] On the whole, the semi-flexible pavement bearing capacity rapid recovery geopolymer grouting material of the present invention has the remarkable characteristics of rapid repair and high early strength, and meets the requirements of the specification, has good high temperature stability, and is also relatively excellent in water stability, and can play a good crack resistance in actual use. And because the aqueous polyurethane emulsion can synergize with inorganic substances, there are two functional groups of affinity for organic and affinity for inorganic in the molecule, which builds a bridge between inorganic and organic materials, and can increase the bonding strength between materials. At the same time, the aqueous polyurethane emulsion condenses together to dehydrate and form a film, and interweaves with the gel product and the unhydrated powder particles to form a mesh structure. While rapidly repairing, the material structure is made denser and the early strength is higher. From the data of the implementation of the regulations, the present invention not only meets the requirements of conventional engineering for grouting materials, but also consumes less energy and discharges less waste. At the same time, due to the rapid repair and high early strength of the grouting material, the construction time is reduced, and the green and sustainable development of the grouting material is achieved. With the promotion of the polymer grouting material for rapid recovery of semi-flexible pavement bearing capacity of the present invention, not only can the pollution caused by the use of cement-based grouting materials to the environment be greatly reduced, but also the pavement performance can be excellent when used in actual construction. At the same time, in actual construction, combined with the designed fixed-point repair process, it can improve the construction efficiency while ensuring the construction quality, improve the bearing capacity of the semi-flexible pavement, and meet the requirements of safety and environmental protection.
[0043] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Without departing from the scope and technical principles of the described embodiments, many modifications and changes are obvious to those of ordinary skill in the art, and these modifications and changes should also be regarded as the scope of protection of the present invention.
Claims
1. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity, characterized in that: The invention is formed by mixing the following raw materials in parts by weight: 57-63 parts of fly ash, 38-42 parts of blast furnace slag, 10-30 parts of sand, 3-9 parts of admixture, 43-48 parts of water and 65-70 parts of alkali activator; the admixture comprises 1-3 parts of waterborne polyurethane emulsion, 1-3 parts of water reducing agent and 1-3 parts of shrinkage reducing agent, the molecular weight of the waterborne polyurethane emulsion is 5000-10000, the alkali activator is a mixture of water glass and sodium hydroxide, and the alkali equivalent is 6%.
2. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The solid content of the aqueous polyurethane emulsion is 30%.
3. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The water reducer is a high-concentration naphthalene-based water reducer.
4. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The shrinkage reducing agent is a polycarboxylic acid high efficiency shrinkage reducing agent.
5. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The sand is standard sand with a particle size of 0.15 mm to 1.18 mm.
6. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The specific surface area of the fly ash is 0.314m 2 / g, the specific surface area of blast furnace slag is 0.428m 2 / g.
7. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 1, characterized in that: The alkaline activator is a mixture of solid sodium hydroxide and water glass, wherein the solid sodium hydroxide is flaky solid particles with a purity of 99%, and the molecular formula of the water glass is Na2O·nSiO2.
8. A geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 7, characterized in that: The modulus of the water glass in the alkali activator is 2.0-2.
5.
9. A method for preparing a geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in any one of claims 1 to 8, characterized in that: The following steps are included: (1) 57-63 parts of fly ash and 38-42 parts of blast furnace slag are uniformly dry-mixed for 30 seconds to obtain a powder; (2) Weigh 10-30 parts of sand, dry-mix the powder and sand evenly for 30 seconds to obtain a solid mixture, and pre-weigh 43-48 parts of water; (3) Preparation of alkaline activator: Add sodium hydroxide and water glass to water and stir evenly to prepare an alkaline activator with an alkali equivalent of 4% to 7% and a water glass modulus of 2.0 to 2.5, and let it stand for 24 hours; (4) adding 1-3 parts of aqueous polyurethane emulsion, 1-3 parts of water reducing agent, 1-3 parts of shrinkage reducing agent, 65-70 parts of alkali activator and remaining water to 95-105 parts of solid mixture and slowly stirring for 120 seconds to prepare a gel material; (5) The cementitious material is finally rapidly stirred for 120 seconds to obtain a geopolymer grouting material for rapid recovery of the bearing capacity of a semi-flexible pavement.
10. A fixed-point repair process using the geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity according to claim 1, characterized in that: The steps include: Step 1: Material selection and ratio optimization; Step 2: Base cleaning, drilling layout, static pressure grouting and grouting pressure control during construction; Step three: real-time monitoring of grouting in quality control, measurement of pavement deflection after grouting, geological radar detection, and maintenance of the construction area; Step 4: Construction safety management and environmental protection; The first step of the process is to select, optimize the proportion and prepare the geopolymer grouting material for rapid recovery of the bearing capacity of the semi-flexible pavement; Step 2 of the process is base cleaning, drilling layout, static pressure grouting and grouting pressure control during the construction process. Among them, base cleaning requires thorough cleaning of the semi-rigid base to remove loose materials and impurities to ensure the cleanliness and dryness of the grouting area. The drilling layout needs to be based on the road conditions and the deflection basin index (BDI) analysis results, and the drilling positions and spacings should be reasonably arranged to ensure that the grouting material can effectively penetrate into the defective areas of the base. The static pressure method is used for grouting. The condition of insufficient density is simulated by reducing the number of compaction times. Then, polymer penetration grouting is carried out to test its bearing capacity and analyze the feasibility of polymer penetration grouting. The pressure is controlled not to exceed 0.3MPa during the grouting process to prevent damage to the surrounding structures.
11. A fixed-point repair process of geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 10, characterized in that: Step three of the process is to monitor the grouting pressure, grouting volume and grouting depth in real time during quality control to ensure the construction quality, measure the pavement deflection value and conduct geological radar detection after the grouting is completed, and maintain the construction area.
12. A fixed-point repair process of a geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity as claimed in claim 10, characterized in that: Step 4 of the process is construction safety management and environmental protection. Safety regulations are strictly observed during the construction process, and measures are taken to reduce dust and noise pollution during the construction process to protect the surrounding environment.
13. The fixed-point repair process of a geopolymer grouting material for rapid recovery of semi-flexible pavement bearing capacity according to claim 10, characterized in that: The supporting construction methods and equipment can maximize the bearing capacity of the semi-flexible pavement. The prepared polymer grouting material for rapid recovery of the bearing capacity of the semi-flexible pavement has an injection rate of 90%, a 7d compressive strength ≥15MPa, a 28d compressive strength ≥30MPa, a 7d shrinkage rate ≤0.3%, and a low-temperature beam maximum bending tensile strain ≥1500με.