Component determination method of ammonia alkali white mud baking-free brick and preparation method of baking-free brick
By determining the component ratio and modification treatment of ammonia alkali white mud, combining slag, fly ash, slag and other materials, the vibration pressing process is used to prepare ammonia alkali white mud without burning bricks, which solves the resource consumption and solid waste in the existing technology. The problem of low utilization rate has achieved efficient utilization of ammonia alkali white mud and the strength improvement of bricks.
Patent Information
- Application Number
- CN202411159107.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing fire-free bricks consume a large amount of natural resources and emit carbon dioxide during the firing process. The ammonia alkali white mud is low in water content and high chloride ion content, low market acceptance and low industrial solid waste utilization rate, resulting in waste of resources and environment. pollute.
By determining the component ratio and modification treatment of ammonia alkali white mud, combining slag, fly ash, slag and other solid waste materials, the vibration pressing molding process is used to prepare ammonia alkali white mud without burning bricks, adjust the moisture content and pH value, and stimulate the The activity of slag and fly ash produces hydration products, reduces curing time, and achieves 100% industrial solid waste utilization.
It improves the physical and chemical effects of ammonia alkali white mud, reduces drying costs, saves water resources, enhances the strength and utilization rate of bricks, reduces resource waste and environmental pollution, and improves the comprehensive utilization efficiency of industrial solid waste.
Smart Images

Figure BDA0005005931440000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of solid waste treatment, and particularly relates to a method for determining the components of an ammonia-alkali white mud unfired brick and a method for preparing the unfired brick. Background Art
[0002] Unburned bricks are a new type of wall material that is made by mechanical equipment vibration pressing and curing without high-temperature calcination. It has the characteristics of high solid waste utilization rate. my country's infrastructure projects are large-scale, and civil engineering, transportation engineering, etc. have a huge demand for brick products. At present, unburned bricks mainly use cement as a binder. However, the process of burning cement clinker will emit a large amount of carbon dioxide and consume a lot of natural resources.
[0003] Ammonia-soda mud is a solid waste generated in the process of producing soda ash by the ammonia-soda process. It is mainly composed of minerals such as sulfates, carbonates, and chlorides. It can be used as a raw material for the preparation of building materials, but due to its high water content and high chloride ion content, it will have potential harm to the durability of the structure when used in cement concrete, and the market acceptance is low. In addition, my country's bulk industrial solid waste such as slag, fly ash, tailings, steel slag, slag, etc. has a large stock, and the overall utilization rate is low. Large-scale accumulation causes waste of resources and environmental pollution. Summary of the invention
[0004] The embodiment of the present invention provides a method for determining the components of an ammonia-soda mud unfired brick and a method for preparing the unfired brick, aiming to prepare an ammonia-soda mud unfired brick with high market acceptance by utilizing solid waste raw materials such as ammonia-soda mud, slag, furnace slag, and fly ash.
[0005] In the first aspect, in order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is: to provide a method for determining the components of ammonia-alkali white mud unfired bricks, the method comprising:
[0006] Step 1, testing the moisture content ω1 of the modified ammonia-soda white mud;
[0007] Step 2, determine the modified ammonia-alkali white mud and the amount of water used, the modified ammonia-alkali white mud X = 20 / (1-ω1) ~ 40 / (1-ω1) parts, water Y = (20-ω1X) ~ (50-ω1X);
[0008] Step 3: Calculate Y-ω1X according to the moisture content of the modified ammonia-soda white mud. When Y-ω1X≥0, determine the composition of each component according to ①; when Y-ω1X<0, determine the composition of each component according to ②;
[0009] ① By mass, the components are as follows: modified ammonia-soda mud X=20 / (1-ω1)~40 / (1-ω1) parts, mineral powder 10~20 parts, fly ash 0~10 parts, slag 10~40 parts, aggregate 15~35 parts, water Y=(20-ω1X)~(50-ω1X) parts;
[0010] ② Dry the modified ammonia-alkali white mud to a moisture content of ω2, so that Y-ω2X ≥ 0; at this time, its components are composed of: dried modified ammonia-alkali white mud X = 20 / (1-ω2) ~ 40 / (1-ω2) parts, mineral powder 10 to 20 parts, fly ash 0 to 10 parts, slag 10 to 20 parts, aggregate 15 to 25 parts, water Y = (20-ω2X) ~ (50-ω2X) parts.
[0011] In combination with the first aspect, in one achievable manner, the method for preparing the modified ammonia-soda white mud comprises:
[0012] Step 1: According to the moisture content of the ammonia-soda mud, the mass ratio of the dry ammonia-soda mud to water is adjusted to 1:5-10 by adding distilled water or drying to obtain a mixed slurry; after stirring with a stirrer at a speed of 350-450 r / min for 5-8 minutes, the mixture is allowed to stand for 0.5-1 hour; during the period, the mixed slurry is heated in a water bath to maintain the temperature of 20-30° C.;
[0013] Step 2: Maintain the temperature at 20-30°C, continue to stir the mixed slurry at 350-450 r / min, and measure the pH value in real time using a pH meter; slowly add a 400m 2 / kg~500m 2 / kg of steel slag powder, until the pH reaches 11.5-12.5; record the amount of steel slag powder added at this time, and calculate the mass ratio m of the steel slag powder to the ammonia-soda white mud;
[0014] Step 3: Mix ammonia-soda white mud and steel slag powder in a mass ratio of 1:m, and grind them together in a ball mill by wet grinding to a specific surface area of 450m 2 / kg~550m 2 / kg, to obtain modified ammonia-soda white mud.
[0015] In combination with the first aspect, in a feasible manner, the ammonia-soda white mud is solid waste generated in the process of producing soda ash using the ammonia-soda method using raw salt, limestone and coke as raw materials, and the chemical components include CaCO3 35% to 60%, CaCl2 5% to 15%, CaSO4 5% to 20%, Ca(OH)2 2% to 12%, MgO2% to 12%, SiO2 0% to 10%, and others 0% to 10%, and the particle size is 0 to 50 μm.
[0016] In combination with the first aspect, in one achievable manner, the ore powder is a molten material composed of silicate and aluminosilicate obtained by quenching and granulating during smelting pig iron in a blast furnace, and the powdery material obtained after grinding has a specific surface area of 450 to 500 m 2 / kg, 28d activity ≥95%.
[0017] In combination with the first aspect, in one achievable manner, the fly ash is fine ash collected from flue gas after coal combustion.
[0018] In combination with the first aspect, in one achievable manner, the slag is solid waste generated during the coal combustion process of a circulating fluidized bed boiler, and has a particle size of 0 to 10 mm.
[0019] In combination with the first aspect, in one achievable manner, the aggregate is at least one of steel slag, coal gangue, and tailings; and the particle size of the steel slag, coal gangue, and tailings is 2 to 10 mm.
[0020] In a second aspect, an embodiment of the present invention further provides a method for preparing an unfired brick, based on the components determined by the method for determining the components of an ammonia-alkali white mud unfired brick, the method for preparing an unfired brick comprises:
[0021] Step 1: put mineral powder, fly ash, modified ammonia-alkali white mud and water into the equipment according to the mass ratio and stir for 3 minutes to obtain a uniform slurry;
[0022] Step 2, adding slag and aggregate into the slurry prepared in step 1 according to the mass ratio, stirring for 2 to 5 minutes to obtain wet brick material;
[0023] Step 3, placing the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick;
[0024] Step 4, demoulding the formed bricks and curing them to a specified age to obtain ammonia-alkali white mud unfired bricks.
[0025] In combination with the second aspect, in one feasible method, vibration and pressing are carried out simultaneously, with a vibration time of 3s to 5s, a holding time of 5s to 8s, a vibration frequency of 3000Hz to 3500Hz, and a molding pressure of 10MPa to 15MPa.
[0026] In combination with the second aspect, in one achievable method, in step four, the demolding time is 24h to 48h after molding, the curing time is 28d, the curing temperature is 15°C to 25°C, and the curing humidity is ≥80%.
[0027] Compared with the prior art, the method for determining the components of the ammonia-soda white mud unfired brick and the method for preparing the unfired brick provided by the present invention have the following beneficial effects:
[0028] (1) The physical and chemical effects of ammonia-alkali mud can be fully exerted. By adding steel slag to modify the ammonia-alkali mud and adjusting the pH value, the alkaline components and sulfate components of the ammonia-alkali mud can work together with the CaO component in the steel slag to stimulate the activity of slag and fly ash to generate hydrated calcium silicate and hydrated calcium aluminosilicate, which provide the strength of unfired bricks. The fine calcium carbonate in the ammonia-alkali mud can act as a crystal nucleus to promote the formation of hydration products. The chloride salt in the ammonia-alkali mud can react with the active substances in the ore powder and fly ash to generate C3A·CaCl2·10H2O, which has an early strength effect on unfired bricks and reduces the curing time of unfired bricks.
[0029] (2) Ammonia-soda mud has a high moisture content and usually needs to be dried before it can be recycled, which results in high resource utilization costs. The present invention can fully utilize the moisture in the modified ammonia-soda mud by calculating the moisture content and target water consumption, thereby eliminating the need for drying or reducing the drying process and saving water resources.
[0030] (3) The alkaline components in the original slag can promote the activity of mineral powder and fly ash, and at the same time can play the role of aggregate, transmitting pressure during pressure molding, and overcoming the uneven density and air holding stratification caused by finer mixtures such as ammonia-alkali white mud.
[0031] (4) Aggregates are selected from bulk industrial solid wastes such as tailings, coal gangue, and steel slag, so as to achieve 100% utilization of industrial solid wastes to prepare unburned bricks and improve the comprehensive utilization efficiency of industrial solid wastes. DETAILED DESCRIPTION
[0032] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0033] Example 1
[0034] 1. Preparation of modified ammonia-alkali white mud:
[0035] Step 1: Take 100g of ammonia-soda mud, and measure the water content of ammonia-soda mud to be 58%, that is, the mass ratio of dry ammonia-soda mud to water is 42:58, add 194g of distilled water, and adjust the mass ratio of dry ammonia-soda mud to water to 1:6. Get a mixed slurry, stir it at a speed of 400r / min for 5min with a stirrer, and let it stand for 0.5h. During this period, use a water bath to heat the mixed slurry to maintain it at 25°C.
[0036] Step 2: Continue stirring the mixed slurry at 400 r / min at 25°C, and measure the pH value in real time using a pH meter. Slowly add a 410 m 2 / kg of steel slag powder was added until the pH reached 11.8. The amount of steel slag powder added at this time was recorded as 18g, and the mass ratio m to ammonia-soda white mud was 0.18.
[0037] Step 3: Mix ammonia-soda white mud and steel slag powder in a mass ratio of 1:0.18, and grind them together in a ball mill by wet grinding to a specific surface area of 480m 2 / kg, to obtain modified ammonia-soda white mud.
[0038] 2. Determine the composition of each component.
[0039] Step 1: The moisture content of the modified ammonia-alkali white mud is measured to be 38%.
[0040] Step 2: by mass, 26 / (1-ω1) parts of modified ammonia-alkali white mud and 32-ω1X parts of water.
[0041] Step three, after verification, 32-[0.38×26 / (1-0.38)]=16.1>0, according to ①, the composition of each part is determined as follows: 42 parts of modified ammonia-alkali white mud, 12 parts of mineral powder, 0 parts of fly ash, 10 parts of slag, 20 parts of aggregate, and 16 parts of water.
[0042] 3. Ammonia-soda white mud is the solid waste generated in the process of producing soda ash using the ammonia-soda method, using raw salt, limestone and coke as raw materials. Its main chemical components are CaCO3 52%, CaCl2 10%, CaSO4 13%, Ca(OH)2 6%, MgO6%, SiO2 8%, and others 5%, with a particle size of 0 to 50 μm.
[0043] 4. Ore powder is a molten material with silicate and aluminosilicate as the main components obtained after quenching and granulation during the smelting of pig iron in a blast furnace. It is a powdery material obtained after grinding. The specific surface area is 470m 2 / kg, activity 105% at 28 days.
[0044] 5. Fly ash is the fine ash collected from the flue gas after coal combustion, which meets the requirements of Class II F ash index in GB / T1596-2017 "Fly ash used in cement and concrete".
[0045] 6. Slag is a solid waste produced during the coal combustion process of a circulating fluidized bed boiler, with a particle size of 0 to 10 mm.
[0046] 7. Aggregate is made of steel slag and tailings in a mass ratio of 1:1. The particle size is 2 to 10 mm.
[0047] 8. A method for preparing unburned bricks by using ammonia-alkali white mud, comprising the following steps:
[0048] Step 1: Put mineral powder, fly ash, modified ammonia-alkali white mud and water into the equipment according to weight proportion and stir for 3 minutes to obtain a uniform slurry.
[0049] First add the mineral powder, fly ash and ammonia-alkali white mud and stir them, which will help to evenly disperse the powder materials and help ensure the uniformity of the mixture during the subsequent addition of aggregates.
[0050] Step 2: Add slag and aggregate into the slurry prepared in step 1 according to weight ratio, stir for 2 minutes, and obtain wet brick material.
[0051] Step three, putting the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick.
[0052] In this process, vibration and pressing are carried out simultaneously. Vibration can ensure the compactness of the brick, and pressing can ensure the strength of the brick. The vibration time is 3s, the pressure holding time is 6s, the vibration frequency is 3000Hz, and the molding pressure is 10.0MPa.
[0053] Step 4, demoulding the formed bricks and curing them to a specified age to obtain ammonia-alkali white mud unfired bricks.
[0054] The demoulding time is 24 hours after molding, the curing time is 28 days, the curing temperature is 18°C, and the curing humidity is 95%.
[0055] Example 2
[0056] 1. Preparation of modified ammonia-alkali white mud:
[0057] Step 1: Take 100g of ammonia-soda mud, and measure the water content of ammonia-soda mud to be 46%, that is, the mass ratio of dry ammonia-soda mud to water is 54:46, add 386g of distilled water, and adjust the mass ratio of dry ammonia-soda mud to water to 1:8. Get a mixed slurry, stir it at 400r / min for 5min with a stirrer, and let it stand for 0.5h. During this period, use a water bath to heat the mixed slurry to maintain it at 25°C.
[0058] Step 2: Continue stirring the mixed slurry at 400 r / min at 25°C, and measure the pH value in real time using a pH meter. Slowly add a 460 m 2 / kg of steel slag powder was added until the pH reached 12.1. The amount of steel slag powder added at this time was recorded as 31g, and the mass ratio m to ammonia-soda white mud was 0.31.
[0059] Step 3: Mix ammonia-soda white mud and steel slag powder in a mass ratio of 1:0.31, and grind them together in a ball mill by wet grinding to a specific surface area of 510m 2 / kg, to obtain modified ammonia-soda white mud.
[0060] 2. Determine the composition of each component.
[0061] Step 1: The moisture content of the modified ammonia-alkali white mud is measured to be 36%.
[0062] Step 2: by mass, 30 / (1-ω1) parts of modified ammonia-alkali white mud and 27 / (1-ω1) parts of water Y=27-ω1X parts.
[0063] Step three, after verification, 27-[0.36×30 / (1-0.36)]=10.1>0, according to ①, the composition of each part is determined as follows: 47 parts of modified ammonia-alkali white mud, 12 parts of mineral powder, 2 parts of fly ash, 12 parts of slag, 17 parts of aggregate, and 10 parts of water.
[0064] 3. Ammonia-soda white mud is the solid waste generated in the process of producing soda ash using the ammonia-soda method, using raw salt, limestone and coke as raw materials. Its main chemical components are CaCO3 46%, CaCl2 8%, CaSO4 16%, Ca(OH)2 5%, MgO7%, SiO2 9%, and others 9%, with a particle size of 0 to 50 μm.
[0065] 4. Ore powder is a molten material with silicate and aluminosilicate as the main components obtained after quenching and granulation during the smelting of pig iron in a blast furnace. It is a powdery material obtained after grinding with a specific surface area of 500m 2 / kg, activity 105% at 28 days.
[0066] 5. Fly ash is the fine ash collected from the flue gas after coal combustion, which meets the requirements of Class II F ash index in GB / T1596-2017 "Fly ash used in cement and concrete".
[0067] 6. Slag is a solid waste produced during the coal combustion process of a circulating fluidized bed boiler, with a particle size of 0 to 10 mm.
[0068] 7. Aggregate is made of coal gangue and tailings in a mass ratio of 1:1. The particle size is 2 to 10 mm.
[0069] 8. A method for preparing unburned bricks by using ammonia-alkali white mud, comprising the following steps:
[0070] Step 1: Put mineral powder, fly ash, modified ammonia-alkali white mud and water into the equipment according to weight proportion and stir for 3 minutes to obtain a uniform slurry.
[0071] First add the mineral powder, fly ash and ammonia-alkali white mud and stir them, which will help to evenly disperse the powder materials and help ensure the uniformity of the mixture during the subsequent addition of aggregates.
[0072] Step 2: Add slag and aggregate into the slurry prepared in step 1 according to weight ratio, stir for 2 minutes, and obtain wet brick material.
[0073] Step three, putting the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick.
[0074] In this process, vibration and pressing are carried out simultaneously. Vibration can ensure the compactness of the brick, and pressing can ensure the strength of the brick. The vibration time is 4s, the pressure holding time is 8s, the vibration frequency is 3200Hz, and the molding pressure is 14.0MPa.
[0075] Step 4, demoulding the formed bricks and curing them to a specified age to obtain ammonia-alkali white mud unfired bricks.
[0076] The demoulding time is 48h after molding, the curing time is 28d, the curing temperature is 22℃, and the curing humidity is 95%.
[0077] Example 3
[0078] 1. Preparation of modified ammonia-alkali white mud:
[0079] Step 1: Take 100g of ammonia-soda mud, and measure the water content of ammonia-soda mud to be 63%, that is, the mass ratio of dry ammonia-soda mud to water is 37:63, add 196g of distilled water, and adjust the mass ratio of dry ammonia-soda mud to water to 1:7. Get a mixed slurry, stir it at 400r / min for 5min with a stirrer, and let it stand for 0.5h. During this period, use a water bath to heat the mixed slurry to maintain it at 25°C.
[0080] Step 2: Continue stirring the mixed slurry at 400 r / min at 25°C and measure the pH value in real time using a pH meter. Slowly add a 500 m 2 / kg of steel slag powder was added until the pH reached 12.3. The amount of steel slag powder added at this time was recorded as 28g, and the mass ratio m to ammonia-soda white mud was 0.28.
[0081] Step 3: Mix ammonia-soda white mud and steel slag powder in a mass ratio of 1:0.28, and grind them together in a ball mill by wet grinding to a specific surface area of 500m 2 / kg, to obtain modified ammonia-soda white mud.
[0082] 2. Determine the composition of each component.
[0083] Step 1: The moisture content of the modified ammonia-alkali white mud is measured to be 41%.
[0084] Step 2: by mass, 35 / (1-ω1) parts of modified ammonia-alkali white mud and 22-ω1X parts of water.
[0085] Step three, it has been verified that 22-[0.41×35 / (1-0.41)]=-2.3<0, according to ②, the modified ammonia-alkali white mud is dried to a moisture content ω2 of 36%, and the composition of each part is determined as: modified ammonia-alkali white mud 35 / (1-ω2)=55 parts, mineral powder 14 parts, fly ash 2 parts, slag 10 parts, aggregate 17 parts, and water 2 parts.
[0086] 3. Ammonia-soda white mud is the solid waste generated in the process of producing soda ash using the ammonia-soda method, using raw salt, limestone and coke as raw materials. Its main chemical components are CaCO3 51%, CaCl2 8%, CaSO4 15%, Ca(OH)2 6%, MgO4%, SiO2 10%, and others 6%, with a particle size of 0 to 50 μm.
[0087] 4. Ore powder is a molten material with silicate and aluminosilicate as the main components obtained after quenching and granulation during the smelting of pig iron in a blast furnace. It is a powdery material obtained after grinding. The specific surface area is 515m 2 / kg, activity 104% at 28 days.
[0088] 5. Fly ash is the fine ash collected from the flue gas after coal combustion, which meets the requirements of Class II F ash index in GB / T1596-2017 "Fly ash used in cement and concrete".
[0089] 6. Slag is a solid waste produced during the coal combustion process of a circulating fluidized bed boiler, with a particle size of 0 to 10 mm.
[0090] 7. Aggregate is made of steel slag, coal gangue and tailings in a mass ratio of 1:1:2. The particle size is 2 to 10 mm.
[0091] 8. A method for preparing unburned bricks by using ammonia-alkali white mud, comprising the following steps:
[0092] Step 1: Put mineral powder, fly ash, modified ammonia-alkali white mud and water into the equipment according to weight proportion and stir for 3 minutes to obtain a uniform slurry.
[0093] First add the mineral powder, fly ash and ammonia-alkali white mud and stir them, which will help to evenly disperse the powder materials and help ensure the uniformity of the mixture during the subsequent addition of aggregates.
[0094] Step 2: Add slag and aggregate into the slurry prepared in step 1 according to weight ratio, stir for 2 minutes, and obtain wet brick material.
[0095] Step three, putting the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick.
[0096] In this process, vibration and pressing are carried out simultaneously. Vibration can ensure the compactness of the brick, and pressing can ensure the strength of the brick. The vibration time is 4s, the pressure holding time is 6s, the vibration frequency is 3300Hz, and the molding pressure is 12.0MPa.
[0097] Step 4, demoulding the formed bricks and curing them to a specified age to obtain ammonia-alkali white mud unfired bricks.
[0098] The demoulding time is 48h after molding, the curing time is 28d, the curing temperature is 21°C, and the curing humidity is 95%.
[0099] Comparative Example 1
[0100] Calculated by mass percentage, the raw materials are: 15 parts of ordinary Portland cement, 51 parts of recycled aggregate from construction waste (chemical composition and technical indicators are shown in Table 1 and Table 2), 19 parts of iron tailings, and 15 parts of water.
[0101] Table 1 Chemical composition of recycled aggregate from construction waste
[0102] <![CDATA[SiO2]]> CaO <![CDATA[Al2O3]]> <![CDATA[Fe2O3]]> MgO <![CDATA[K2O]]> <![CDATA[SO3]]> <![CDATA[Na2O]]> <![CDATA[TiO2]]> 48.14 23.90 13.84 5.32 3.17 2.43 1.33 1.12 0.76
[0103] Table 2 Technical indicators of recycled aggregate from construction waste
[0104] Gradation / mm <![CDATA[Apparent density / (kg / m 3 )]]> <![CDATA[Apparent density / (kg / m 3 )]]> Water absorption / % Crushing index / % 10~20 1439.7 2682.5 3.1 16.3
[0105] The preparation method comprises the following steps:
[0106] Step 1: Put ordinary Portland cement and water in a certain weight ratio into the equipment and stir for 3 minutes to obtain a uniform slurry.
[0107] First add ordinary Portland cement and water and stir, which will help to evenly disperse the powder material and help ensure the uniformity of the mixture during the subsequent addition of aggregate.
[0108] Step 2: Add construction waste recycled aggregate and iron tailings into the slurry prepared in step 1 according to weight ratio, stir for 2 minutes, and obtain wet brick material.
[0109] Step three, putting the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick.
[0110] In this process, vibration and pressing are carried out simultaneously. Vibration can ensure the compactness of the brick, and pressing can ensure the strength of the brick. The vibration time is 3s, the pressure holding time is 6s, the vibration frequency is 3000Hz, and the molding pressure is 10.0MPa.
[0111] Step 4: demoulding the formed bricks and curing them to a specified age to obtain cement unfired bricks.
[0112] The demoulding time is 24 hours after molding, the curing time is 28 days, the curing temperature is 18°C, and the curing humidity is 95%.
[0113] The material performance index data of the unfired bricks made in the above Examples 1-3 and Comparative Example 1 were tested for the performance of unfired bricks according to GB / T2542-2012 "Test Methods for Wall Bricks". After experimental testing, the test results are shown in Table 3.
[0114] Table 3
[0115]
[0116]
[0117] According to the experimental test data in the above table, the utilization rate of ammonia-alkali white mud for preparing unfired bricks in the present invention is high, and the compressive strength, post-freezing compressive strength and post-carbonization compressive strength are better than those of current unfired bricks. At the same time, compared with other existing reported documents (Document 1: CN 106986592 A "A method for making bricks from alkali slag sludge", Document 2: CN 118206358 A "A road brick and its preparation method"; Document 3: CN 102161579A "A unfired and steamed alkali slag brick and its preparation method"), the utilization rate of ammonia-alkali white mud in the present invention is higher, so the unfired bricks prepared by the present invention have better performance and higher absorption capacity of ammonia-alkali white mud per unit mass.
[0118] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for determining the components of ammonia-soda white mud unfired bricks, characterized in that: The method comprises: Step 1, testing the moisture content ω1 of the modified ammonia-soda white mud; Step 2, determine the modified ammonia-alkali white mud and the amount of water used, the modified ammonia-alkali white mud X = 20 / (1-ω1) ~ 40 / (1-ω1) parts, water Y = (20-ω1X) ~ (50-ω1X); Step 3: Calculate Y-ω1X according to the moisture content of the modified ammonia-soda white mud. When Y-ω1X≥0, determine the composition of each component according to ①; when Y-ω1X<0, determine the composition of each component according to ②; ① By mass, the components are as follows: modified ammonia-soda mud X=20 / (1-ω1)~40 / (1-ω1) parts, mineral powder 10~20 parts, fly ash 0~10 parts, slag 10~40 parts, aggregate 15~35 parts, water Y=(20-ω1X)~(50-ω1X) parts; ② Dry the modified ammonia-alkali white mud to a moisture content of ω2, so that Y-ω2X ≥ 0; at this time, its components are composed of: dried modified ammonia-alkali white mud X = 20 / (1-ω2) ~ 40 / (1-ω2) parts, mineral powder 10 to 20 parts, fly ash 0 to 10 parts, slag 10 to 20 parts, aggregate 15 to 25 parts, water Y = (20-ω2X) ~ (50-ω2X) parts.
2. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 1, characterized in that: The preparation method of the modified ammonia-soda white mud comprises: Step 1: According to the moisture content of the ammonia-soda mud, the mass ratio of the dry ammonia-soda mud to water is adjusted to 1:5-10 by adding distilled water or drying to obtain a mixed slurry; after stirring with a stirrer at a speed of 350-450 r / min for 5-8 minutes, the mixture is allowed to stand for 0.5-1 hour; during the period, the mixed slurry is heated in a water bath to maintain the temperature of 20-30° C.; Step 2: Maintain the temperature at 20-30°C, continue to stir the mixed slurry at 350-450 r / min, and measure the pH value in real time using a pH meter; slowly add a 400m 2 / kg~500m 2 / kg of steel slag powder, until the pH reaches 11.5-12.5; record the amount of steel slag powder added at this time, and calculate the mass ratio m of the steel slag powder to the ammonia-soda white mud; Step 3: Mix ammonia-soda white mud and steel slag powder in a mass ratio of 1:m, and grind them together in a ball mill by wet grinding to a specific surface area of 450m 2 / kg~550m 2 / kg, to obtain modified ammonia-soda white mud.
3. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 2, characterized in that: The ammonia-soda white mud is solid waste generated in the process of producing soda ash by the ammonia-soda method using raw salt, limestone and coke as raw materials. The chemical components include CaCO3 35%-60%, CaCl2 5%-15%, CaSO4 5%-20%, Ca(OH)2 2%-12%, MgO 2%-12%, SiO2 0%-10%, and others 0%-10%, and the particle size is 0-50μm.
4. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 1, characterized in that: The ore powder is a molten material composed of silicate and aluminosilicate obtained by quenching and granulation during blast furnace smelting of pig iron. The powdery material has a specific surface area of 450-500m 2 / kg, 28d activity ≥95%.
5. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 1, characterized in that: The fly ash is fine ash collected from the flue gas after coal combustion.
6. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 1, characterized in that: The slag is solid waste generated during the coal burning process of a circulating fluidized bed boiler, and has a particle size of 0 to 10 mm.
7. The method for determining the components of ammonia-soda white mud unfired bricks according to claim 1, characterized in that: The aggregate is at least one of steel slag, coal gangue and tailings; the particle sizes of steel slag, coal gangue and tailings are all 2-10 mm.
8. A method for preparing unfired bricks, based on the components determined by the method for determining the components of ammonia-soda white mud unfired bricks according to any one of claims 1 to 7, characterized in that: The method for preparing the unburned brick comprises: Step 1: put mineral powder, fly ash, modified ammonia-alkali white mud and water into the equipment according to the mass ratio and stir for 3 minutes to obtain a uniform slurry; Step 2, adding slag and aggregate into the slurry prepared in step 1 according to the mass ratio, stirring for 2 to 5 minutes to obtain wet brick material; Step 3, placing the wet brick material into a vibration pressing and molding device, and pressing and molding to obtain a molded brick; Step 4, demoulding the formed bricks and curing them to a specified age to obtain ammonia-alkali white mud unfired bricks.
9. The method for preparing unburned bricks according to claim 8, characterized in that: In step three, vibration and pressing are carried out simultaneously, with a vibration time of 3s to 5s, a holding time of 5s to 8s, a vibration frequency of 3000Hz to 3500Hz, and a molding pressure of 10MPa to 15MPa.
10. The method for preparing unburned bricks according to claim 8, characterized in that: In step 4, the demoulding time is 24h to 48h after molding, the curing time is 28d, the curing temperature is 15°C to 25°C, and the curing humidity is ≥80%.
Citation Information
Patent Citations
Burning-and-steam-curing-free alkaline slag brick and preparation method thereof
CN102161579A
Alkaline slag sludge brick making method
CN106986592A
Walking brick and preparation method thereof
CN118206358A