Alkali-activated dispersed curing agent based on clay geology and preparation method thereof
The alkali-excited dispersed curing agent is prepared by using ordinary silicate cement, fast penetrant T50, organically modified calcium carbonate, sodium silicate and sodium hexametaphosphate, which solves the problems of clay stability and energy consumption. , achieves the improvement of clay strength, durability and stability, is suitable for a variety of clay types, and reduces production costs and environmental pressure.
Patent Information
- Application Number
- CN202410950873.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-12
AI Technical Summary
When existing alkali excitants improve clay strength and durability, they often reduce their stability, and the production process consumes high energy and cost, puts pressure on the environment, and have poor adaptability.
The alkali-exciting dispersed curing agent is prepared by low-energy-consuming mixing and stirring method to improve clay Strength, durability and stability.
It effectively improves the strength, durability and stability of clay, reduces production costs, and reduces energy consumption. It is suitable for various types of clay, and is in line with the development trend of green and environmental protection.
Smart Images

Figure CN118930165A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of curing agents, and in particular to an alkali-activated dispersed curing agent based on clay geology and a preparation method thereof. Background Art
[0002] Clay is a common geological material with good plasticity and adhesion, and is widely used in infrastructure construction such as buildings, roads, and bridges. However, the natural characteristics of clay also cause some problems in its use, such as easy deformation, low strength, and poor durability. In order to solve these problems, the method of adding a curing agent is usually adopted to improve the strength, stability, and durability of the clay by changing its physical and chemical properties. Among them, alkali activator is a commonly used curing agent, which can react with silicates in clay to generate silicate minerals with high strength and stability, thereby improving the performance of clay.
[0003] Existing alkali activators mainly generate solidified soil with a certain strength by adding cement, lime and other materials through hydration reaction. However, this method has some problems in practical application, such as unstable solidification effect, insufficient strength and durability of solidified soil, and easy to be affected by environmental factors. In addition, existing alkali activators are often expensive, which also limits their application in large-scale projects.
[0004] Existing alkali activators tend to reduce the stability of clay while improving its strength and durability. This is because the hydration reaction of the alkali activator changes the structure of the clay, making it more susceptible to environmental factors. In addition, the preparation process of existing alkali activators often requires the use of a large amount of energy and resources, which not only increases production costs, but also puts a certain amount of pressure on the environment. Therefore, how to prepare an alkali-activated dispersed curing agent that can effectively improve the strength, durability and stability of clay solidified bodies under low energy consumption and environmentally friendly conditions is a problem that needs to be solved urgently in this field. Summary of the invention
[0005] Based on the above content, the present invention provides an alkali-activated dispersed curing agent based on clay geology and a preparation method thereof. The present invention prepares an alkali-activated dispersed curing agent that effectively improves the strength, durability and stability of clay under low energy consumption and environmentally friendly conditions.
[0006] To achieve the above object, the present invention provides the following solutions:
[0007] One of the technical solutions of the present invention is an alkali-activated dispersed curing agent based on clay geology, wherein the raw materials include, by weight: 90-92 parts of ordinary Portland cement, 0.5-1 parts of rapid penetrant, 3-5 parts of organic modified calcium carbonate, 0.05-0.1 parts of sodium silicate and 0.03-0.05 parts of sodium hexametaphosphate.
[0008] The second technical solution of the present invention is a method for preparing the above-mentioned alkali-activated dispersed curing agent based on clay geology, which comprises uniformly mixing the raw materials according to their mass fractions to obtain the alkali-activated dispersed curing agent based on clay geology.
[0009] A third technical solution of the present invention is the use of the above-mentioned alkali-activated dispersed curing agent based on clay geology in curing clay.
[0010] A fourth technical solution of the present invention is a method for improving the strength, durability and stability of clay, which improves the strength, durability and stability of clay by adding the above-mentioned alkali-activated dispersed curing agent based on clay geology to the clay.
[0011] The present invention discloses the following technical effects:
[0012] 1. The alkali-activated dispersed curing agent based on clay geology of the present invention can effectively improve the strength, durability and stability of clay through a specific raw material composition, solving the problem of unstable curing effect of curing agents and insufficient strength and durability of cured soil in the prior art.
[0013] 2. The alkali-activated dispersed curing agent based on clay geology of the present invention uses ordinary Portland cement, rapid penetrant T50, organic modified calcium carbonate, sodium silicate and sodium hexametaphosphate as raw materials. These raw materials are widely available and inexpensive, which is conducive to reducing production costs and solves the problem of high production costs in the prior art.
[0014] 3. The alkali-activated dispersed curing agent based on clay geology of the present invention is suitable for various types of clay, has strong adaptability and practicality, and solves the problem of poor adaptability of curing agents in the prior art.
[0015] 4. The preparation method of the alkali-activated dispersed curing agent based on clay geology of the present invention does not require high temperature and high pressure conditions, and only needs to be mixed and stirred at room temperature, which greatly reduces production energy consumption and reduces pressure on the environment. It is in line with the current development trend of green environmental protection and solves the problem of high energy consumption and pressure on the environment in the prior art. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1The present invention is a flow chart of curing clay with an alkali-activated dispersed curing agent based on clay geology. DETAILED DESCRIPTION
[0018] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0019] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0020] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0021] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0022] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0023] The "room temperature" described in the present invention, unless otherwise specified, refers to 20-30°C.
[0024] The "%" described in the present invention, unless otherwise specified, refers to mass percentage.
[0025] The first aspect of the present invention provides an alkali-activated dispersed curing agent based on clay geology. The raw materials include, by weight: 90-92 parts of ordinary Portland cement, 0.5-1 parts of rapid penetrant, 3-5 parts of organic modified calcium carbonate, 0.05-0.1 parts of sodium silicate and 0.03-0.05 parts of sodium hexametaphosphate.
[0026] In the present invention, the addition of organic modified calcium carbonate promotes cement hydration and improves hydration efficiency on the one hand, but too much addition will make the hydration exothermic reaction more intense, and uncontrollable factors will appear, which will have a serious impact on the stability of the solidified soil. On the other hand, the organic modified calcium carbonate plays the role of micro-aggregate, fills the voids, and increases the packing density, which helps to improve the flexural and compressive strengths. However, adding too much will cause the organic modified calcium carbonate to accumulate alone, and its structural strength is far less than that of other large particles, resulting in a decrease in the overall strength.
[0027] In the present invention, sodium silicate can form colloidal SiO2 during cement hydration, which can block capillary pores and play an anti-seepage role. However, too much sodium silicate will cause the cement to solidify and harden too quickly, and a large amount of gas cannot be discharged, thereby reducing the strength of the solidified soil.
[0028] In the present invention, sodium hexametaphosphate contains a large amount of phosphate ions, which can form stable calcium phosphate substances, react with cement to form hydrated calcium phosphate, thereby enhancing the strength and durability of cement. However, if the amount of sodium hexametaphosphate added is too much, it will cause the early strength of cement to decrease, and even cause stratification, separation and other phenomena.
[0029] If the above three raw materials (organic modified calcium carbonate, sodium silicate and sodium hexametaphosphate) are added too little (below the parameter range specified in the present invention), the cement hydration efficiency will be reduced, the early strength will increase slowly, and the strength at the end of the age will be lower than the cement strength with the addition amount specified in the present invention.
[0030] In some embodiments of the present invention, the ordinary Portland cement is PO 42.5.
[0031] In some embodiments of the present invention, the fast penetrant is fast penetrant T50.
[0032] In some embodiments of the present invention, the particle size of the organically modified calcium carbonate is 0.5-1.0 μm.
[0033] The particle size of organically modified calcium carbonate exceeding the above parameter range will lead to a significant decrease in the hydration rate, greatly prolonging the initial and final setting time of the cement, and the excessively large particle size will greatly weaken its own micro-aggregate effect, increase the voids, and greatly reduce the packing density compared to the above particle size range.
[0034] In some embodiments of the present invention, the modulus of the sodium silicate is 1.2-2.3.
[0035] As one of the two activators, sodium silicate has a too small modulus and provides very few silicate ions, so double excitation becomes single excitation and the improvement of cement strength is not significant. If the modulus is too large, the sodium silicate activator provides too high a concentration of silicate ions. Because the polymerization degree of silicate anions themselves increases, it becomes difficult to react with calcium ions, resulting in a decrease in cement strength.
[0036] In the invention, ordinary Portland cement is selected as the main raw material to provide basic cementitious material.
[0037] In the invention, the rapid penetrant T50 is added to improve the dispersibility and permeability of the curing agent in the clay, thereby improving the curing effect.
[0038] In the invention, organic modified calcium carbonate is added to improve the strength and stability of the solidified soil.
[0039] In the invention, sodium silicate with a modulus of 1.2-2.3 is added as an alkali activator to increase the hydration activity of the cementitious material, thereby improving the strength and durability of the solidified soil.
[0040] In the present invention, sodium hexametaphosphate is added as another alkali activator to work together with sodium silicate to further improve the hydration activity of the cementitious material, thereby improving the strength and durability of the solidified soil.
[0041] The curing agent of the present invention is applied to clay geology, and the strength, durability, stability and other properties of the premixed fluidized solidified soil are effectively improved through the hydration catalysis of the gelling material by the alkaline activator.
[0042] The second aspect of the present invention provides a method for preparing the above-mentioned alkali-activated dispersible curing agent based on clay geology, comprising uniformly mixing the raw materials according to their mass fractions to obtain the above-mentioned alkali-activated dispersible curing agent based on clay geology.
[0043] In some embodiments of the present invention, a three-dimensional mixer for powder materials or a cement mortar mixer may be used to mix the raw materials at room temperature for 30 minutes to obtain the alkali-activated dispersed curing agent based on clay geology.
[0044] The third aspect of the present invention provides a use of the above-mentioned alkali-activated dispersed curing agent based on clay geology in curing clay.
[0045] A fourth aspect of the present invention provides a method for improving the strength, durability and stability of clay, wherein the strength, durability and stability of the clay are improved by adding the above-mentioned alkali-activated dispersible curing agent based on clay geology to the clay.
[0046] In some embodiments of the present invention, the mass ratio of the clay-based alkali-activated dispersed curing agent to the clay is 1:10.
[0047] In some embodiments of the present invention, after adding the clay-based alkali-activated dispersed curing agent to the clay, a step of mixing for 15 minutes is further included. The mixing is performed using a cement mortar mixer.
[0048] The present invention prepares a curing agent that can effectively improve the strength, durability and stability of clay under low energy consumption and environmentally friendly conditions; the present invention optimizes the formula of the alkali activator to improve its curing effect on clay and improve the performance of the cured soil; the present invention reduces the production cost of the alkali activator and reduces its pressure on the environment.
[0049] The flow chart of the present invention for curing clay using an alkali-activated dispersed curing agent based on clay geology is as follows Figure 1 shown.
[0050] Unless otherwise specified, the raw materials used in the embodiments of the present invention can be obtained through commercial sources.
[0051] The ordinary Portland cement used in the embodiments of the present invention is PO 42.5.
[0052] The active ingredient content of the fast penetrant T50 used in the embodiment of the present invention is 98%.
[0053] The organic modified calcium carbonate used in the embodiment of the present invention is XFC-10-F3 organic modified calcium carbonate produced by Quanzhou Xufeng Powder Raw Material Co., Ltd., with a calcium content of ≥97% and a particle size of 0.5 μm.
[0054] The modulus of the sodium silicate used in the embodiment of the present invention is 1.8.
[0055] The purity of the sodium hexametaphosphate used in the embodiment of the present invention is 98%.
[0056] The present invention is further described below by way of examples.
[0057] Example 1
[0058] The invention discloses an alkali-activated dispersed curing agent based on clay geology. The raw materials thereof are composed of 90 parts of ordinary Portland cement, 0.5 parts of rapid penetrant T50, 3 parts of organic modified calcium carbonate, 0.05 parts of sodium silicate and 0.03 parts of sodium hexametaphosphate in parts by weight.
[0059] The preparation method of the above-mentioned alkali-activated dispersed curing agent based on clay geology comprises the following steps: mixing the raw materials uniformly according to their mass fractions (using a cement mortar mixer to mix at room temperature for 30 minutes) to obtain an alkali-activated dispersed curing agent based on clay geology (abbreviated as: curing agent).
[0060] Application Example 1
[0061] The curing agent prepared in Example 1 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0062] Example 2
[0063] The invention discloses an alkali-activated dispersed curing agent based on clay geology. The raw materials thereof are composed of 90 parts of ordinary Portland cement, 0.5 parts of rapid penetrant T50, 3 parts of organic modified calcium carbonate, 0.1 parts of sodium silicate and 0.03 parts of sodium hexametaphosphate in parts by weight.
[0064] The preparation method of the above-mentioned alkali-activated dispersed curing agent based on clay geology comprises the following steps: mixing the raw materials uniformly according to their mass fractions (using a cement mortar mixer to mix at room temperature for 30 minutes) to obtain an alkali-activated dispersed curing agent based on clay geology (abbreviated as: curing agent).
[0065] Application Example 2
[0066] The curing agent prepared in Example 2 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0067] Example 3
[0068] The invention discloses an alkali-activated dispersed curing agent based on clay geology. The raw materials thereof are composed of 90 parts of ordinary Portland cement, 0.5 parts of rapid penetrant T50, 3 parts of organic modified calcium carbonate, 0.05 parts of sodium silicate and 0.05 parts of sodium hexametaphosphate in parts by weight.
[0069] The preparation method of the above-mentioned alkali-activated dispersed curing agent based on clay geology comprises the following steps: mixing the raw materials uniformly according to their mass fractions (using a cement mortar mixer to mix at room temperature for 30 minutes) to obtain an alkali-activated dispersed curing agent based on clay geology (abbreviated as: curing agent).
[0070] Application Example 3
[0071] The curing agent prepared in Example 3 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0072] Example 4
[0073] The invention discloses an alkali-activated dispersed curing agent based on clay geology. The raw materials thereof are composed of 90 parts of ordinary Portland cement, 0.5 parts of rapid penetrant T50, 3 parts of organic modified calcium carbonate, 0.1 parts of sodium silicate and 0.05 parts of sodium hexametaphosphate in parts by weight.
[0074] The preparation method of the above-mentioned alkali-activated dispersed curing agent based on clay geology comprises the following steps: mixing the raw materials uniformly according to their mass fractions (using a cement mortar mixer to mix at room temperature for 30 minutes) to obtain an alkali-activated dispersed curing agent based on clay geology (abbreviated as: curing agent).
[0075] Application Example 4
[0076] The curing agent prepared in Example 4 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0077] Example 5
[0078] The only difference from Example 4 is that the addition of sodium hexametaphosphate is omitted and the addition amount of sodium silicate is 0.15 parts.
[0079] Application Example 5
[0080] The curing agent prepared in Example 5 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0081] Example 6
[0082] The only difference from Example 4 is that the addition of sodium silicate is omitted and the addition amount of sodium hexametaphosphate is 0.15 parts.
[0083] Application Example 6
[0084] The curing agent prepared in Example 6 was mixed with clay in a mass ratio of 1:10, the mixing time was 15 minutes, the mixing temperature was room temperature, and the mixing equipment was a cement mortar mixer to obtain premixed fluidized solidified soil (abbreviated as: solidified soil).
[0085] According to the liquid limit and plastic limit test method in the "Standard for Geotechnical Test Methods" (GB / T 50123-2019), the liquid limit, plastic limit, plasticity index and seven-day unconfined compressive strength of the original clay and consolidated soil in Application Examples 1-6 were tested, and the results are shown in Table 1.
[0086] Table 1
[0087]
[0088]
[0089] It can be seen from the data in Table 1 that after adding sodium silicate and sodium hexametaphosphate to the curing agent, the liquid limit and plastic limit index of the clay are greatly reduced, the ability of the soil to bind water is weakened, and the deformation resistance is enhanced, which significantly improves the water stability and compressive strength of the clay. The reason why the test parameters of Application Example 3 are higher than those of Application Example 2 can be analyzed as follows: compared with silicic acid, the two alkaline activators sodium silicate and sodium hexametaphosphate have more hydrogen ions in the phosphoric acid molecule than silicic acid, and can undergo more dissociation reactions with water molecules, and the generated ion effect is stronger than that of silicic acid. At the same time, the sum of the electronegativity of the phosphorus atom and the oxygen atom in the phosphoric acid molecule is higher than that of silicic acid, which can attract more electrons to obtain negative charges from water molecules, further improving the hydration activity of the cement, thereby improving the strength and durability of the cured soil.
[0090] From the effect data of Application Example 4, it can be seen that when the two alkaline activators, sodium silicate and sodium hexametaphosphate, are at high content, their combined effect is stronger, which effectively improves the strength, durability and stability of the clay.
[0091] Comparing the effect data of Application Examples 5, 6 and 4, it can be seen that the effect of a single alkali activator with a high content is not as good as the effect of a combination of two alkali activators, sodium silicate and sodium hexametaphosphate, and the effect of sodium hexametaphosphate is stronger than that of sodium silicate.
[0092] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.
Claims
1. An alkali-activated dispersed curing agent based on clay geology, characterized in that: Calculated by weight, the raw materials include: 90-92 parts of ordinary Portland cement, 0.5-1 parts of rapid penetrant, 3-5 parts of organic modified calcium carbonate, 0.05-0.1 parts of sodium silicate and 0.03-0.05 parts of sodium hexametaphosphate.
2. The alkali-activated dispersible curing agent based on clay geology according to claim 1, characterized in that: The ordinary Portland cement is PO 42.5 or PO 52.
5.
3. The alkali-activated dispersible curing agent based on clay geology according to claim 1, characterized in that: The particle size of the organic modified calcium carbonate is 0.5-1.0 μm.
4. A method for preparing an alkali-activated dispersed curing agent based on clay geology according to any one of claims 1 to 3, characterized in that: The raw materials are uniformly mixed according to their mass fractions to obtain the alkali-activated dispersed curing agent based on clay geology.
5. Use of the alkali-activated dispersed curing agent based on clay geology as claimed in any one of claims 1 to 3 in curing clay.
6. A method for improving the strength, durability and stability of clay, characterized in that: The strength, durability and stability of the clay are improved by adding the clay-based alkali-activated dispersed curing agent according to any one of claims 1 to 3 to the clay.
7. The method for improving the strength, durability and stability of clay according to claim 6, characterized in that: The mass ratio of the clay-based alkali-activated dispersed curing agent to the clay is 1:
10.
8. The method for improving the strength, durability and stability of clay according to claim 6, characterized in that: After adding the clay-based alkali-activated dispersed curing agent to the clay, the step of mixing for 15 minutes is also included.
Citation Information
Cited By
Solid waste low-carbon flow-state solidified soil dry-mixed curing agent as well as preparation method and application thereof
CN121609522A