Constant-temperature curing-free concrete and preparation method thereof

By using composite moisturizers with triethanolamine borate, hydroxyethylurea, sodium pyrophosphate and polyoxyethylene glycerol ether in concrete, the problem of constant temperature maintenance in large cast-in-place concrete projects is solved, and high The concrete curing effect of strength is suitable for large-scale projects.

CN118930187APending Publication Date: 2024-11-12广东东方混凝土有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196528.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Large cast-in-place concrete projects are difficult to achieve constant temperature maintenance, resulting in low concrete strength and affecting the quality of the project.

Method used

The composite moisturizer is used to combine triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate, and polyoxyethylene glycerol ether to control the hydration rate by locking water and slowly releasing moisture, and improve the hydration degree and strength of concrete. High strength can still be achieved after the constant temperature maintenance process is cancelled.

Benefits of technology

Without constant temperature curing, the strength of concrete is significantly improved and is suitable for large cast-in-place concrete projects, ensuring construction quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of concrete materials, and particularly discloses constant-temperature curing-free concrete and a preparation method thereof. The constant-temperature curing-free concrete comprises the following components in parts by mass: 100 parts of water; 255 to 260 parts of cement; 28 to 29 parts of fly ash; 450 to 460 parts of fine aggregate; 625 to 635 parts of coarse aggregate; 30 to 34 parts of a composite humectant; 4.4 to 4.8 parts of an auxiliary agent; the composite humectant is formed by compounding triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glyceryl ether. The method has the advantage that the concrete can still obtain higher strength without a constant-temperature curing process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of concrete materials, and in particular to a constant temperature curing-free concrete and a preparation method thereof. Background Art

[0002] Concrete is one of the main modern building materials. It is mainly made of a mixture of cementitious materials, aggregates, admixtures and water. Concrete has good fluidity before solidification and high strength after solidification, which makes concrete widely used.

[0003] The concrete curing process is the hydration reaction process of cementitious materials. During the hydration process, if the ambient temperature is too high or too dry, it will cause excessive evaporation of water in the concrete, resulting in a lack of water in the concrete for hydration reaction, which will lead to insufficient hydration reaction of the concrete, and then cause a significant decrease in the strength of the concrete. Therefore, constant temperature maintenance is generally required during the concrete construction process to maintain a constant temperature and humidity to reduce the loss of water in the concrete, thereby ensuring the strength of the concrete after curing.

[0004] However, the constant temperature curing process is complicated, and constant temperature curing is difficult to achieve for large-scale cast-in-place concrete projects, which results in the strength of large-scale cast-in-place concrete being easily low, affecting the quality of the project. Therefore, there is still room for improvement. Summary of the invention

[0005] In order to enable concrete to obtain high strength without the need for constant temperature curing process, the present application provides concrete without the need for constant temperature curing and a preparation method thereof.

[0006] In the first aspect, the present application provides a constant temperature curing-free concrete, which adopts the following technical solution: A constant temperature curing-free concrete comprising the following components in parts by mass: 100 parts water; 255-260 parts of cement; Fly ash 28-29 parts; 450-460 parts of fine aggregate; 625-635 parts of coarse aggregate; 30-34 parts of composite moisturizer; 4.4-4.8 parts of additives; The composite moisturizing agent is a compound of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether.

[0007] By adopting the above technical scheme, by adding a composite moisturizer composed of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether into concrete, the cement slurry has a good water-locking effect, so that water and cement are evenly dispersed, and water is not easy to lose, and the composite moisturizer can also slowly release water, thereby realizing the control of hydration rate, so that the hydration degree is high, the strength of the cured concrete is significantly improved, and after canceling the constant temperature curing process, a high strength level can still be achieved, so that the concrete can be well used in large-scale cast-in-place concrete projects.

[0008] Preferably, the mass ratio of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether is 6-7:9-10:3-4:12-13.

[0009] By adopting the above technical scheme and specifically selecting the mass ratio of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether, the composite moisturizing agent has a better moisturizing effect, can better reduce water evaporation, can achieve a higher degree of hydration reaction, and can increase the strength of the concrete after curing and provide better quality.

[0010] Preferably, the auxiliary agent is a compound of a water reducer and a retarder.

[0011] By adopting the above technical solution, the processing performance of concrete is improved, and under the action of the retarder, the concrete has sufficient stirring time, so that the composite moisturizing agent can be evenly dispersed in the concrete, so that the water-locking and moisturizing effect is better, thereby making the concrete more hydrated and stronger.

[0012] Preferably, the mass ratio of the water reducer to the retarder is 3.1-3.3:1.3-1.5.

[0013] By adopting the above technical solution and specifically selecting the mass ratio of the water reducer and the retarder, the effect of improving the processing performance of the concrete mixture is better, and there is more sufficient time for mixing, so that the concrete has higher strength and better quality after curing.

[0014] Preferably, the water reducer is a polycarboxylate water reducer.

[0015] By adopting the above technical solution and specifically selecting the polycarboxylate water-reducing agent, the water-reducing effect is better, the dosage is less, and the quality of the concrete after curing is better.

[0016] Preferably, the retarder is sodium gluconate.

[0017] By adopting the above technical solution and specifically selecting sodium gluconate as the retarder, the retarding effect is better, the concrete can be stirred for a longer time, and the composite moisturizing agent can fully exert its effect.

[0018] In a second aspect, the present application provides a method for preparing concrete without constant temperature curing, which adopts the following technical solution: A method for preparing constant temperature curing-free concrete comprises the following steps: Step 1), mixing water and a composite moisturizer uniformly to obtain a premix; Step 2), adding cement, fly ash and additives to the premix, mixing evenly to obtain a mixture; Step 3), adding fine aggregate and coarse aggregate to the mixture, mixing evenly, to obtain a concrete mixture; Step 4), injecting the concrete mixture into the mold and leaving it to solidify, thereby avoiding the need for constant temperature curing of the concrete.

[0019] By adopting the above technical solution, the obtained concrete does not need constant temperature curing and can be left to stand naturally. Moreover, the strength after curing is relatively high and it is not easy to cause strength reduction due to failure to perform constant temperature curing.

[0020] Preferably, in the step 1), during mixing, the speed is first 120-140 r / min, stirring for 5-8 min, and then 2500-3000 r / min, homogenizing for 10-15 min; in the step 2), during mixing, the speed is first 120-140 r / min, stirring for 3-5 min, and then 2500-3000 r / min, homogenizing for 20-25 min.

[0021] By adopting the above technical solution, the composite moisturizing agent is evenly dispersed in the cement slurry through sufficient stirring and homogenization, so that the composite moisturizing agent can fully exert its effect, the hydration reaction of the concrete is more complete, and the strength of the cured concrete is higher.

[0022] In summary, this application has the following beneficial effects: 1. Since the present application adds a composite moisturizer composed of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether into concrete, the cement slurry has a good water-locking effect, so that water and cement are evenly dispersed, and water is not easy to lose. In addition, the composite moisturizer can slowly release water, thereby achieving the control of hydration rate, so that the hydration degree is high, and the strength of the cured concrete is significantly improved. After canceling the constant temperature curing process, a high strength level can still be achieved, so that the concrete can be well applied to large-scale cast-in-place concrete projects.

[0023] 2. In the present application, it is preferred to specifically select the mass ratio of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether so that the composite moisturizing agent has a better moisturizing effect, reduces water evaporation better, and makes the degree of hydration reaction higher, so that the strength of the concrete after curing is higher and the quality is better. DETAILED DESCRIPTION

[0024] The present application is further described in detail below in conjunction with embodiments.

[0025] Example 1 A constant temperature curing-free concrete comprising the following components: Water, cement, fly ash, fine aggregate, coarse aggregate, composite moisturizer, additives.

[0026] The cement is ordinary Portland cement, Runfeng cement, factory standard: PO 42.5R.

[0027] The fly ash is first-grade fly ash, which is commercially available.

[0028] Fine aggregate is natural river sand, sourced from the market, 3-5 mm.

[0029] The coarse aggregate is basalt crushed stone, which is commercially available and has a size of 12-15 mm.

[0030] The additive is a compound of water reducer and retarder.

[0031] The water reducer is a polycarboxylate water reducer purchased from Nanjing Xinyi Synthetic Technology Co., Ltd., model: 1200.

[0032] The retarder is sodium gluconate purchased from Suzhou Wujiang District Xingsheng Chemical Technology Co., Ltd.

[0033] The composite moisturizer is a compound of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether.

[0034] Triethanolamine borate is commercially available, CAS number: 283-56-7.

[0035] Hydroxyethyl urea is commercially available, CAS number: 2078-71-9.

[0036] Sodium pyrophosphate is commercially available, CAS number: 7722-88-5.

[0037] Polyoxyethylene glycerol ether is commercially available, CAS number: 32694-55-0.

[0038] The method for preparing concrete without constant temperature curing is characterized by comprising the following steps: Step 1), 100 kg of water, 6 kg of triethanolamine borate, 9 kg of hydroxyethyl urea, 3 kg of sodium pyrophosphate, and 12 kg of polyoxyethylene glycerol ether are put into a stirring tank, the speed is 120 r / min, stirred for 5 min, and then 2500 r / min, homogenized for 10 min to obtain a premix.

[0039] Step 2), add 255kg cement, 28kg fly ash, 3.1kg polycarboxylate water reducer, 1.3kg sodium gluconate to the premix, stir at a speed of 120r / min for 3min, then at 2500r / min, homogenize for 20min to obtain a mixture.

[0040] Step 3), add 450kg of fine aggregate and 625kg of coarse aggregate into the mixture, rotate at 60r / min, stir for 10min, and obtain concrete mixture.

[0041] Step 4), inject the concrete mixture into the mold, let it stand for 7 days, demould, and let it stand until the 28th day, so that the concrete can be cured at a constant temperature.

[0042] Example 2 A constant temperature curing-free concrete comprising the following components: Water, cement, fly ash, fine aggregate, coarse aggregate, composite moisturizer, additives.

[0043] The cement is ordinary Portland cement, Runfeng cement, factory standard: PO 42.5R.

[0044] The fly ash is first-grade fly ash, which is commercially available.

[0045] Fine aggregate is natural river sand, sourced from the market, 3-5 mm.

[0046] The coarse aggregate is basalt crushed stone, which is commercially available and has a size of 12-15 mm.

[0047] The additive is a compound of water reducer and retarder.

[0048] The water reducer is a polycarboxylate water reducer purchased from Nanjing Xinyi Synthetic Technology Co., Ltd., model: 1200.

[0049] The retarder is sodium gluconate purchased from Suzhou Wujiang District Xingsheng Chemical Technology Co., Ltd.

[0050] The composite moisturizer is a compound of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether.

[0051] Triethanolamine borate is commercially available, CAS number: 283-56-7.

[0052] Hydroxyethyl urea is commercially available, CAS number: 2078-71-9.

[0053] Sodium pyrophosphate is commercially available, CAS number: 7722-88-5.

[0054] Polyoxyethylene glycerol ether is commercially available, CAS number: 32694-55-0.

[0055] The method for preparing concrete without constant temperature curing is characterized by comprising the following steps: Step 1), 100 kg of water, 6.5 kg of triethanolamine borate, 9.5 kg of hydroxyethyl urea, 3.5 kg of sodium pyrophosphate, and 12.5 kg of polyoxyethylene glycerol ether are put into a stirring tank, the speed is 130 r / min, stirring for 6.5 min, and then 2800 r / min, homogenizing for 12.5 min to obtain a premix.

[0056] Step 2), add 258kg cement, 285kg fly ash, 3.2kg polycarboxylate water reducer, 1.4kg sodium gluconate to the premix, stir at a speed of 130r / min for 4min, then at 2800r / min, homogenize for 22.5min to obtain a mixture.

[0057] Step 3), add 455kg of fine aggregate and 630kg of coarse aggregate into the mixture, rotate at 65r / min, stir for 12.5min, and obtain concrete mixture.

[0058] Step 4), inject the concrete mixture into the mold, let it stand for 7 days, demould, and let it stand until the 28th day, so that the concrete can be cured at a constant temperature.

[0059] Example 3 A constant temperature curing-free concrete comprising the following components: Water, cement, fly ash, fine aggregate, coarse aggregate, composite moisturizer, additives.

[0060] The cement is ordinary Portland cement, Runfeng cement, factory standard: PO 42.5R.

[0061] The fly ash is first-grade fly ash, which is commercially available.

[0062] Fine aggregate is natural river sand, sourced from the market, 3-5 mm.

[0063] The coarse aggregate is basalt crushed stone, which is commercially available and has a size of 12-15 mm.

[0064] The additive is a compound of water reducer and retarder.

[0065] The water reducer is a polycarboxylate water reducer purchased from Nanjing Xinyi Synthetic Technology Co., Ltd., model: 1200.

[0066] The retarder is sodium gluconate purchased from Suzhou Wujiang District Xingsheng Chemical Technology Co., Ltd.

[0067] The composite moisturizer is a compound of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether.

[0068] Triethanolamine borate is commercially available, CAS number: 283-56-7.

[0069] Hydroxyethyl urea is commercially available, CAS number: 2078-71-9.

[0070] Sodium pyrophosphate is commercially available, CAS number: 7722-88-5.

[0071] Polyoxyethylene glycerol ether is commercially available, CAS number: 32694-55-0.

[0072] The method for preparing concrete without constant temperature curing is characterized by comprising the following steps: Step 1), 100 kg of water, 7 kg of triethanolamine borate, 10 kg of hydroxyethyl urea, 4 kg of sodium pyrophosphate, and 13 kg of polyoxyethylene glycerol ether are put into a stirring tank, the speed is 140 r / min, stirring for 8 min, and then 3000 r / min, homogenizing for 15 min to obtain a premix.

[0073] Step 2), add 260kg cement, 29kg fly ash, 3.3kg polycarboxylate water reducer, 1.5kg sodium gluconate to the premix, stir at a speed of 140r / min for 5min, then at 3000r / min, homogenize for 25min to obtain a mixture.

[0074] Step 3), add 460kg fine aggregate and 635kg coarse aggregate into the mixture, rotate at 70r / min, stir for 15min, and obtain concrete mixture.

[0075] Step 4), inject the concrete mixture into the mold, let it stand for 7 days, demould, and let it stand until the 28th day, so that the concrete can be cured at a constant temperature.

[0076] Comparative Example 1 A constant temperature curing-free concrete, compared with Example 2, the only difference is: In the composite moisturizer, triethanolamine is used in an equal amount to replace triethanolamine borate.

[0077] Triethanolamine is commercially available, CAS number: 102-71-6.

[0078] Comparative Example 2 A constant temperature curing-free concrete, compared with Example 2, the only difference is: In the composite moisturizer, 1,3-butanediol is used to replace hydroxyethyl urea in equal amounts.

[0079] 1,3-Butanediol is commercially available, CAS No.: 107-88-0.

[0080] Comparative Example 3 A constant temperature curing-free concrete, compared with Example 2, the only difference is: In the composite moisturizer, tricalcium phosphate is used to replace sodium pyrophosphate in equal amounts.

[0081] Tricalcium phosphate is commercially available, CAS number: 7758-87-4.

[0082] Comparative Example 4 A constant temperature curing-free concrete, compared with Example 2, the only difference is: In the composite moisturizer, triglycerol is used to replace polyoxyethylene glyceryl ether in equal amounts.

[0083] Triglycerol is commercially available, CAS number: 56090-54-1.

[0084] Comparative Example 5 A constant temperature curing-free concrete, compared with Example 2, the only difference is: In the composite moisturizer, triethanolamine is used in an equal amount to replace triethanolamine borate; 1,3-butanediol is used in an equal amount to replace hydroxyethyl urea; tricalcium phosphate is used in an equal amount to replace sodium pyrophosphate; and triglycerol is used in an equal amount to replace polyoxyethylene glyceryl ether.

[0085] Triethanolamine is commercially available, CAS number: 102-71-6.

[0086] 1,3-Butanediol is commercially available, CAS No.: 107-88-0.

[0087] Tricalcium phosphate is commercially available, CAS number: 7758-87-4.

[0088] Triglycerol is commercially available, CAS number: 56090-54-1.

[0089] Comparative Example 6 A constant temperature curing concrete, comprising the following components: Water, cement, fly ash, fine aggregate, coarse aggregate, additives.

[0090] The cement is ordinary Portland cement, Runfeng cement, factory standard: PO 42.5R.

[0091] The fly ash is first-grade fly ash, which is commercially available.

[0092] Fine aggregate is natural river sand, sourced from the market, 3-5 mm.

[0093] The coarse aggregate is basalt crushed stone, which is commercially available and has a size of 12-15 mm.

[0094] The additive is a compound of water reducer and retarder.

[0095] The water reducer is a polycarboxylate water reducer purchased from Nanjing Xinyi Synthetic Technology Co., Ltd., model: 1200.

[0096] The retarder is sodium gluconate purchased from Suzhou Wujiang District Xingsheng Chemical Technology Co., Ltd.

[0097] The method for preparing constant temperature curing concrete is characterized by comprising the following steps: Step 1), 100 kg water, 258 kg cement, 285 kg fly ash, 3.2 kg polycarboxylate water reducer, 1.4 kg sodium gluconate, stirring at a speed of 130 r / min for 4 min, and then homogenizing at 2800 r / min for 22.5 min to obtain a mixture.

[0098] Step 2), add 455kg of fine aggregate and 630kg of coarse aggregate into the mixture, rotate at 65r / min, stir for 12.5min, and obtain concrete mixture.

[0099] Step 3), inject the concrete mixture into the mold, and perform constant temperature curing in a curing room for 7 days, demould, and perform constant temperature curing until the 28th day to obtain constant temperature cured concrete, wherein the temperature in the curing room is 30±1°C and the relative humidity is 90±2%.

[0100] Comparative Example 7 A constant temperature curing-free concrete comprising the following components: Water, cement, fly ash, fine aggregate, coarse aggregate, additives.

[0101] The cement is ordinary Portland cement, Runfeng cement, factory standard: PO 42.5R.

[0102] The fly ash is first-grade fly ash, which is commercially available.

[0103] Fine aggregate is natural river sand, sourced from the market, 3-5 mm.

[0104] The coarse aggregate is basalt crushed stone, which is commercially available and has a size of 12-15 mm.

[0105] The additive is a compound of water reducer and retarder.

[0106] The water reducer is a polycarboxylate water reducer purchased from Nanjing Xinyi Synthetic Technology Co., Ltd., model: 1200.

[0107] The retarder is sodium gluconate purchased from Suzhou Wujiang District Xingsheng Chemical Technology Co., Ltd.

[0108] The method for preparing concrete without constant temperature curing is characterized by comprising the following steps: Step 1), 100 kg water, 258 kg cement, 285 kg fly ash, 3.2 kg polycarboxylate water reducer, 1.4 kg sodium gluconate, stirring at a speed of 130 r / min for 4 min, and then homogenizing at 2800 r / min for 22.5 min to obtain a mixture.

[0109] Step 2), add 455kg of fine aggregate and 630kg of coarse aggregate into the mixture, rotate at 65r / min, stir for 12.5min, and obtain concrete mixture.

[0110] Step 3), inject the concrete mixture into the mold, let it stand for 7 days, demould, and let it stand until the 28th day, so that the concrete can be cured at a constant temperature.

[0111] Experiment 1 According to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 7-day compressive strength and 28-day compressive strength of the concrete samples prepared in each embodiment and comparative example were tested.

[0112] The specific test data of Experiment 1 are shown in Table 1.

[0113] Table 1 7-day compressive strength (MPa) 28-day compressive strength (MPa) Example 1 36.1 49.3 Example 2 36.3 49.6 Example 3 36.5 49.8 Comparative Example 1 31.8 43.4 Comparative Example 2 31.6 43.1 Comparative Example 3 32.2 43.9 Comparative Example 4 31.9 43.5 Comparative Example 5 31.3 42.7 Comparative Example 6 35.3 48.2 Comparative Example 7 28.3 38.6 According to the data comparison of each embodiment and the comparative example in Table 1, it can be obtained that the compressive strength of each embodiment reaches the level of comparative example 6, or even higher than that of comparative example 6. It can be seen that when the composite moisturizer composed of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate, and polyoxyethylene glycerol ether is added to the concrete, the degree of hydration reaction of the concrete is relatively high, and the strength of the concrete can reach the strength level of the concrete without adding the moisturizer and undergoing constant temperature curing, or even be improved.

[0114] Although the compressive strength of Comparative Example 1-5 is higher than that of Comparative Example 7, it is significantly lower than that of Comparative Example 6. It can be seen that although Comparative Examples 1-5 added moisturizers, they destroyed the special compound system of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate, and polyoxyethylene glycerol ether and failed to fully adapt to the complex system of concrete mixtures. Under the premise of no constant temperature maintenance, the effect of improving the strength of concrete is significantly reduced, and it is difficult to reach the level of constant temperature maintenance.

[0115] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A constant temperature curing-free concrete, characterized in that: The composition includes the following components in parts by weight: 100 parts water; 255-260 parts of cement; Fly ash 28-29 parts; 450-460 parts of fine aggregate; 625-635 parts of coarse aggregate; 30-34 parts of composite moisturizer; 4.4-4.8 parts of additives; The composite moisturizing agent is a compound of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether.

2. The constant temperature curing-free concrete according to claim 1, characterized in that: The mass ratio of triethanolamine borate, hydroxyethyl urea, sodium pyrophosphate and polyoxyethylene glycerol ether is 6-7:9-10:3-4:12-13.

3. The constant temperature curing-free concrete according to claim 1, characterized in that: The auxiliary agent is a compound of a water reducing agent and a retarder.

4. The constant temperature curing-free concrete according to claim 3, characterized in that: The mass ratio of the water reducer to the retarder is 3.1-3.3:1.3-1.

5.

5. The constant temperature curing-free concrete according to claim 4, characterized in that: The water reducer is a polycarboxylate water reducer.

6. The constant temperature curing-free concrete according to claim 4, characterized in that: The retarder is sodium gluconate.

7. A method for preparing constant temperature curing-free concrete according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step 1), mixing water and composite moisturizer evenly to obtain a premix; Step 2), adding cement, fly ash and additives to the premix, mixing evenly to obtain a mixture; Step 3), adding fine aggregate and coarse aggregate into the mixture, mixing evenly, and obtaining a concrete mixture; Step 4) Inject the concrete mixture into the mold and let it stand to solidify, thus avoiding the need for constant temperature curing of the concrete.

8. The method for preparing concrete free of constant temperature curing according to claim 7, characterized in that: In the step 1), when mixing, first rotate at 120-140 r / min, stir for 5-8 min, then rotate at 2500-3000 r / min, homogenize for 10-15 min; in the step 2), when mixing, first rotate at 120-140 r / min, stir for 3-5 min, then rotate at 2500-3000 r / min, homogenize for 20-25 min.