Impermeable low-shrinkage inorganic coating and preparation method thereof
By using low-thermal silicate cement, high-magnesium low-thermal silicate cement and gypsum, combined with saponification reaction of glycerol stearate, a dense structure and a hydrophobic film is formed, which solves the problem of rigid waterproof coatings in the face of temperature changes and structural deformation. The leakage and shrinkage problems achieve more efficient waterproofing performance.
Patent Information
- Application Number
- CN202411208158.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-30
AI Technical Summary
Rigid waterproof coatings are prone to leakage and shrinkage cracks when facing temperature changes and structural deformation, lack ductility and adaptability, making it difficult to effectively prevent water corrosion problems in building structures.
Green inorganic materials such as low-thermal silicate cement, high-magnesium low-thermal silicate cement and gypsum are used to combine with saponification reaction of glycerol stearate to form a dense structure and a hydrophobic membrane, which can alleviate shrinkage problems and improve prevention through micro-expansion and hydrophobic properties. Penetration performance.
It effectively avoids the shrinkage problem of coatings, improves the anti-seepage performance and structural density, and improves the durability and waterproof performance of the building.
Smart Images

Figure QLYQS_1 
Figure BDA0005019615630000011 
Figure BDA0005019615630000041
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of inorganic non-metallic materials, and in particular to an anti-permeability and low-shrinkage inorganic coating and a preparation method thereof. Background Art
[0002] Cement concrete is the most widely used building material, making reinforced concrete structures the main structures of most buildings. It is entirely possible for reinforced concrete structures to reach the national standard service life or even longer according to design requirements. However, leakage problems in building structures are common nowadays, and water erosion has seriously affected the durability of buildings. In order to solve the problem of building leakage, in addition to achieving waterproofing through its own dense structure, the use of waterproof coatings is also an effective means.
[0003] The advantages of rigid waterproof coatings over other flexible waterproof coatings are low cost, no toxic or harmful materials, simple construction and good durability. However, rigid waterproof coatings also have certain defects. Rigid waterproof coatings have no ductility, are very sensitive to structural deformation caused by temperature and uneven settlement, and are prone to leakage, shrinkage cracks and other problems. Summary of the invention
[0004] To overcome the above technical defects and shortcomings, the present invention provides an anti-seepage low-shrinkage inorganic coating and a preparation method thereof. The anti-seepage low-shrinkage inorganic coating is made of green inorganic materials, and combines the characteristics of slow hydration of low-heat silicate cement, micro-expansion of high-magnesium low-heat silicate cement, and micro-expansion of calcium sulfonate products formed between gypsum and cement hydration products. The micro-expansion is used to alleviate the shrinkage problem of the material, so that it forms a dense structure, and the stearic acid glycerol undergoes a saponification reaction under alkaline conditions to make it have hydrophobic and anti-seepage properties.
[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0006] The invention discloses an anti-permeability low-shrinkage inorganic coating, comprising the following raw materials in parts by mass:
[0007]
[0008]
[0009] In some embodiments of the present invention, the cement material includes the following components in percentage by mass: 20-35wt% low-heat Portland cement, 30-50wt% high-magnesium low-heat Portland cement, and 20-43wt% rapid-hardening sulphoaluminate cement.
[0010] In some embodiments of the present invention, the mineral composition of the low-heat Portland cement is: 20-35wt% C3S, 40-60wt% C2S, 2-7% C3A, 10-20% C4AF; the mineral composition of the high-magnesium low-heat Portland cement is: 20-35wt% C3S, 35-60wt% C2S, 1-8wt% C3A, 10-25wt% C4AF, and the MgO content is 3-8wt%; the mineral composition of the fast-hardening sulphoaluminate cement is: 50-70wt% C4A3S, 10-35wt% C2S, 3-8wt% C4AF.
[0011] In some embodiments of the present invention, the active mixed material is at least one of silica ash, fly ash, and blast furnace slag powder.
[0012] In some embodiments of the present invention, the gypsum is industrial solid waste phosphogypsum with a specific surface area of 500 to 700 m 2 / kg
[0013] In some embodiments of the present invention, the talcum powder is industrial grade talcum powder with a fineness of 3000 mesh.
[0014] In some embodiments of the present invention, the glyceryl stearate is glyceryl monostearate.
[0015] In some embodiments of the present invention, the additive is at least one of sodium silicate, a defoamer, a water reducer, lithium carbonate, hydroxypropyl methylcellulose, and a redispersible latex powder.
[0016] In some embodiments of the present invention, the hydroxypropyl methylcellulose is hydroxypropyl methylcellulose with a viscosity of 50,000.
[0017] The present invention also discloses a method for preparing an anti-seepage low-shrinkage inorganic coating, comprising the following steps:
[0018] S1. Mix cement material, active mixed material, gypsum, talcum powder and glyceryl stearate uniformly and then ball-mill to obtain powder. Preferably, the ball-milling speed is 200-400 r / s, the ball-milling time is 10-40 min, and the powder particle size is 5-20 μm.
[0019] S2, stirring the powder obtained in S1 and the admixture at a low speed for 60 seconds, adding water and continuing stirring at a low speed for 30 seconds, and finally stirring rapidly for 60 seconds to obtain a mixed slurry, wherein the mass ratio of the powder to water is 1:0.25;
[0020] S3, pouring the mixed slurry into a mold, vibrating and shaping it, curing it, and demoulding it to obtain the anti-seepage low-shrinkage inorganic coating.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention mainly adopts low-heat silicate cement and high-magnesium low-heat silicate cement. Low-heat silicate cement has the characteristics of small shrinkage and low hydration heat. Low hydration heat can alleviate the cracking of the coating. High-magnesium low-heat silicate cement has a micro-expansion effect. The calcium sulfoxide hydration product generated by adding gypsum also has a micro-expansion effect, which effectively avoids the problem of large shrinkage of the coating.
[0023] 2. The present invention selects glyceryl stearate with lipophilicity as a hydrophobic agent. By grinding a gelling material (cement material) and glyceryl stearate together, the surface of the gelling material particles is evenly coated with glyceryl stearate. Under alkaline conditions, glyceryl stearate is hydrated into stearate and glycerol to form a hydrophobic film to achieve an anti-seepage effect. Talcum powder has a certain hydrophobicity. The active mixed material and talcum powder can fill the capillary pores inside the structure, reduce the porosity, form a denser structure inside the coating, and further improve the anti-seepage performance.
[0024] 3. The sodium silicate of the admixture of the present invention is a crystalline admixture, which can prevent moisture and has a certain hydrophobicity. Sodium silicate can be combined with calcium hydroxide to generate insoluble calcium silicate to fill the gaps. The addition of sodium silicate not only improves the anti-seepage performance of the coating, but also has a positive effect on the activity stimulation of the active mixed material. DETAILED DESCRIPTION
[0025] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0026] In the embodiment of the present invention, the mineral composition of low-heat silicate cement is: 20-35wt% C3S, 40-60wt% C2S, 2-7% C3A, 10-20% C4AF; the mineral composition of high-magnesium low-heat silicate cement is: 20-35wt% C3S, 35-60wt% C2S, 1-8wt% C3A, 10-25wt% C4AF, and the MgO content is 3-8wt%; the mineral composition of fast-hardening sulphoaluminate cement is: 50-70wt% C4A3S, 10-35wt% C2S, 3-8wt% C4AF.
[0027] In the embodiment of the present invention, the active mixed material is at least one of silica ash, fly ash and blast furnace slag powder.
[0028] In the embodiment of the present invention, the gypsum is industrial solid waste phosphogypsum with a specific surface area of 500-700m 2 / kg
[0029] In the embodiment of the present invention, the talcum powder is industrial grade talcum powder with a fineness of 3000 mesh.
[0030] In the embodiment of the present invention, glyceryl stearate is glyceryl monostearate.
[0031] In the embodiment of the present invention, the additive is at least one of sodium silicate, a defoamer, a water reducer, lithium carbonate, hydroxypropyl methylcellulose, and a redispersible latex powder.
[0032] In the embodiment of the present invention, the hydroxypropyl methylcellulose is hydroxypropyl methylcellulose with a viscosity of 50,000.
[0033] In an embodiment of the present invention, a method for preparing an anti-seepage low-shrinkage inorganic coating comprises the following steps:
[0034] S1. Mix cement material, active mixed material, gypsum, talcum powder and glyceryl stearate evenly and place them in a ball mill for ball milling at a ball milling speed of 200 to 400 r / s for 10 to 40 min to obtain a powder with a particle size of 5 to 20 μm.
[0035] S2, stirring the powder obtained in S1 and the admixture at a low speed for 60 seconds, adding water and continuing stirring at a low speed for 30 seconds, and finally stirring rapidly for 60 seconds to obtain a mixed slurry, wherein the mass ratio of the powder to water is 1:0.25;
[0036] S3, pouring the mixed slurry into a mold, vibrating and shaping it, curing it, and demoulding it to obtain the anti-seepage low-shrinkage inorganic coating.
[0037] Example 1
[0038] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 1.
[0039] Table 1 Raw material composition of Example 1 anti-seepage low shrinkage inorganic coating
[0040]
[0041] In this embodiment, the cement material includes the following components by mass percentage: 30wt% low-heat silicate cement, 45wt% high-magnesium low-heat silicate cement, and 25wt% rapid-hardening sulphoaluminate cement.
[0042] According to the mass fractions of the raw materials in Table 1, the anti-seepage low-shrinkage inorganic coating #1 was obtained by adopting the preparation method.
[0043] Example 2
[0044] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 2.
[0045] Table 2 Raw material composition of Example 2 anti-seepage low shrinkage inorganic coating
[0046]
[0047] In this embodiment, the cement material includes the following components by mass percentage: 35wt% low-heat silicate cement, 45wt% high-magnesium low-heat silicate cement, and 20wt% rapid-hardening sulphoaluminate cement.
[0048] According to the mass fractions of each raw material in Table 2, the anti-seepage low-shrinkage inorganic coating #2 was obtained by adopting the preparation method.
[0049] Example 3
[0050] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 3.
[0051] Table 3 Raw material composition of Example 3 anti-seepage low shrinkage inorganic coating
[0052]
[0053] In this embodiment, the cement material includes the following components by mass percentage: 20wt% low-heat silicate cement, 50wt% high-magnesium low-heat silicate cement, and 30wt% fast-hardening sulphoaluminate cement.
[0054] According to the mass fractions of each raw material in Table 3, the anti-seepage low-shrinkage inorganic coating #3 was obtained by adopting the preparation method.
[0055] Example 4
[0056] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 4.
[0057] Table 4 Raw material composition of the anti-seepage low shrinkage inorganic coating of Example 4
[0058]
[0059]
[0060] In this embodiment, the cement material includes the following components by mass percentage: 27wt% low-heat silicate cement, 30wt% high-magnesium low-heat silicate cement, and 43wt% rapid-hardening sulphoaluminate cement.
[0061] According to the mass fractions of each raw material in Table 4, the anti-seepage low-shrinkage inorganic coating #4 was obtained by adopting the preparation method.
[0062] Example 5
[0063] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 5.
[0064] Table 5 Raw material composition of Example 5 anti-seepage low shrinkage inorganic coating
[0065]
[0066]
[0067] In this embodiment, the cement material includes the following components by mass percentage: 32wt% low-heat silicate cement, 35wt% high-magnesium low-heat silicate cement, and 33wt% rapid-hardening sulphoaluminate cement.
[0068] According to the mass fractions of each raw material in Table 5, the anti-seepage low-shrinkage inorganic coating #5 was obtained by adopting the preparation method.
[0069] Example 6
[0070] As a preferred embodiment of the present invention, the anti-seepage low-shrinkage inorganic coating disclosed in this embodiment has a raw material composition as shown in Table 6.
[0071] Table 6 Raw material composition of Example 6 anti-seepage low shrinkage inorganic coating
[0072]
[0073] In this embodiment, the cement material includes the following components by mass percentage: 33wt% low-heat silicate cement, 37wt% high-magnesium low-heat silicate cement, and 30wt% rapid-hardening sulphoaluminate cement.
[0074] According to the mass fractions of each raw material in Table 6, the anti-seepage low-shrinkage inorganic coating #6 was obtained by adopting the preparation method.
[0075] Comparative Example 1
[0076] In this comparative example, except that ordinary silicate cement is used to replace low-heat silicate cement and high-magnesium low-heat silicate cement, the rest is the same as Example 1, and a comparative coating #1 is obtained.
[0077] Comparative Example 2
[0078] In this comparative example, except that ordinary silicate hydrophobic agent was used to replace stearic acid glyceryl ester as the hydrophobic agent, the rest was the same as Example 1 to obtain comparative coating #2.
[0079] Comparative Example 3
[0080] In this comparative example, except that sodium silicate is not used as an additive, the rest is the same as Example 1, and a comparative coating #3 is obtained.
[0081] Test Case
[0082] The coatings of Examples 1 to 6 and Comparative Examples 1 to 3 were tested, and the 7d impermeability pressure, 7d tensile bond strength, 3d flexural strength and 3d compressive strength were tested according to the standard "GB 23440-2009". To test the shrinkage performance of inorganic coatings, the present invention refers to the standard "JGJ / T 70-2009", and the mass ratio of coating: sand: water = 1:3:0.35, wherein the sand is ISO standard sand, and the test results are shown in Table 7.
[0083] Table 7 Test results of various coatings
[0084]
[0085] According to Table 7, compared with Comparative Example 1, the coating of the present invention has a smaller 28d shrinkage rate; compared with Comparative Example 2, the coating of the present invention has a higher 7d anti-seepage pressure; compared with Comparative Example 3, the coating of the present invention has higher 3d flexural strength and 3d compressive strength.
[0086] Finally, it should be noted that the above embodiments are only preferred embodiments of the present invention to illustrate the technical solutions of the present invention, rather than limiting them, and certainly not limiting the patent scope of the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. These modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. In other words, any changes or modifications made to the main design concept and spirit of the present invention that have no substantive significance, and the technical problems they solve are still consistent with the present invention, should be included in the protection scope of the present invention. In addition, the direct or indirect application of the technical solutions of the present invention in other related technical fields is also included in the patent protection scope of the present invention.
Claims
1. An anti-seepage and low-shrinkage inorganic coating, It is characterized in that Including the following raw materials by mass:
2. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The cement material comprises the following components by mass percentage: 20-35wt% of low-heat silicate cement, 30-50wt% of high-magnesium low-heat silicate cement, and 20-43wt% of rapid-hardening sulphoaluminate cement.
3. The anti-seepage low shrinkage inorganic coating according to claim 2, It is characterized in that The mineral composition of the low heat silicate cement is: 20-35wt% C 3 S, 40-60wt% C 2 S, 2~7%C 3 A. 10~20%C 4 AF; The mineral composition of high magnesium low heat silicate cement is 20-35wt% C 3 S, 35-60wt% C 2 S, 1-8 wt% C 3 A. 10~25wt%C 4 AF, MgO content is 3-8wt%; the mineral composition of rapid hardening sulphoaluminate cement is: 50-70wt% C 4 A 3 S, 10-35wt%C 2 S, 3-8 wt% C 4 AF.
4. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The active mixed material is at least one of silica ash, fly ash and blast furnace slag powder.
5. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The gypsum is industrial solid waste phosphogypsum with a specific surface area of 500-700m 2 / kg.
6. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The talcum powder is industrial grade talcum powder with a fineness of 3000 meshes.
7. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The stearic acid glyceryl is monostearate glyceryl.
8. The anti-seepage low shrinkage inorganic coating according to claim 1, It is characterized in that The additive is at least one of sodium silicate, a defoamer, a water reducer, lithium carbonate, hydroxypropyl methylcellulose and redispersible latex powder.
9. The anti-seepage low-shrinkage inorganic coating according to claim 8, It is characterized in that The hydroxypropyl methylcellulose is hydroxypropyl methylcellulose with a viscosity of 50,000.
10. A method for preparing an anti-seepage low-shrinkage inorganic coating according to any one of claims 1 to 9, It is characterized in that The following steps are involved: S1. Mix cement material, active mixed material, gypsum, talcum powder and glyceryl stearate uniformly and then ball-mill to obtain powder. Preferably, the ball-milling speed is 200-400 r / s, the ball-milling time is 10-40 min, and the powder particle size is 5-20 μm. S2, stirring the powder obtained in S1 and the admixture at a low speed for 60 seconds, adding water and continuing stirring at a low speed for 30 seconds, and finally stirring rapidly for 60 seconds to obtain a mixed slurry, wherein the mass ratio of the powder to water is 1:0.25; S3, pouring the mixed slurry into a mold, vibrating and shaping it, curing it, and demoulding it to obtain the anti-seepage low-shrinkage inorganic coating.
Citation Information
Patent Citations
High-magnesium minimum-inflation low-heat cement and preparation method thereof
CN102898050A
High-magnesium low-heat anti-cracking cement for hydraulic mass concrete and preparation method of high-magnesium low-heat anti-cracking cement
CN115259783A
Low-heat low-shrinkage Portland cement and preparation method thereof
CN115784646A
High-early-strength low-shrinkage composite Portland cement and preparation method thereof