Ardealite-based grouting material for tunnel engineering and preparation and application thereof
By using phosphogypsum-based grouting materials in tunnel projects, combined with high-strength phosphogypsum, sulfur aluminate cement and other materials, the water resistance and carbon emission problems of grouting materials in tunnel projects are solved, and high-strength and low-carbon are achieved The preparation of grouting material is suitable for tunnel construction in complex environments.
Patent Information
- Application Number
- CN202411109663.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing grouting materials cannot meet the requirements of underwater non-dispersion, high early strength and good working performance in tunnel projects. At the same time, the settling time of grouting materials prepared by sulfoaluminate cement is difficult to control and have high carbon emissions and energy consumption. The poor water resistance of α-phosphorus gypsum limits its large-scale application.
Using phosphogypsum-based grouting material, it is formulated into high-strength and high-density combined materials, including high-strength phosphogypsum, sulfoaluminate cement, fly ash, silica fume, limestone and special dispersants. By adjusting the formula and process steps, Control the settling time and later strength increase, reduce the amount of cement, and improve water resistance.
The phosphogypsum grouting material has good water resistance, high early strength, and continuous increase in later strength, controlled the setting time, reduced the cement usage, achieved the purpose of low-carbon and environmental protection, and is suitable for tunnel construction and promoted waste recycling.
Smart Images

Figure BDA0004991807280000071
Abstract
Description
Technical Field
[0001] The invention relates to a grouting material and preparation and application thereof, in particular to a phosphogypsum-based grouting material for tunnel engineering and preparation and application thereof. Background Art
[0002] Grouting material is a powder material with cementing and curing ability, which is injected into the cracks, fissures, pores and other internal spaces of the tunnel surrounding rock by means of grouting equipment, compressed air or other power. In view of the adverse geological environment such as high ground stress, large deformation of soft rock, seepage (gushing) water, etc. in tunnels, higher requirements are put forward for grouting materials used in tunnel engineering construction.
[0003] At present, conventional grouting materials cannot meet the requirements of underwater non-dispersion, high early strength and good working performance in complex tunnel environments. Many researchers have proposed using sulphoaluminate cement as a cementitious material to prepare early-strength grouting materials, but the setting time of grouting materials prepared with sulphoaluminate cement is difficult to control, and it has high requirements for on-site construction technicians. At the same time, the use of sulphoaluminate grouting materials has not achieved the goal of carbon emission reduction, and CO2 emissions and energy consumption are still very high.
[0004] Phosphogypsum is a heavily polluted solid waste generated during the production of phosphate fertilizers and phosphoric acid. According to the water content, it can be divided into anhydrous phosphogypsum, hemihydrate phosphogypsum and dihydrate phosphogypsum. Hemihydrate phosphogypsum can be divided into α, β and γ types according to the degree of crystallinity. Among them, α hemihydrate phosphogypsum is a high-strength, high-density, high-crystallinity crystal with good physical properties. It is an ideal raw material for preparing high-strength phosphogypsum grouting materials. However, the water resistance of α phosphogypsum is extremely poor, which seriously limits its large-scale application.
[0005] Therefore, the present invention provides a phosphogypsum-based grouting material for tunnel engineering, proposes a practical and feasible technology for utilizing phosphogypsum, and promotes the green, low-carbon and high-quality development of tunnel engineering. Summary of the invention
[0006] In order to solve the above-mentioned technical problems, the present invention provides a phosphogypsum-based grouting material for tunnel engineering, and its preparation and application. The phosphogypsum grouting material prepared by this method has good water resistance, high early strength, continuous increase in later strength, and controllable setting time. It can not only ensure the quality and safety of on-site construction, but also reduce the amount of cement used, thereby achieving the purpose of low carbon and environmental protection.
[0007] One of the technical solutions of the present invention:
[0008] A phosphogypsum-based grouting material for tunnel engineering comprises, by weight, 40-50 parts of high-strength phosphogypsum, 10-15 parts of sulphoaluminate cement, 5-7 parts of fly ash, 6-8 parts of silica fume, 5-6 parts of limestone, 0.1-0.2 parts of an early strength agent and 1-2 parts of a special dispersant.
[0009] Preferably, the aforementioned phosphogypsum-based grouting material for tunnel engineering comprises, by weight, 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of early strength agent and 2 parts of special dispersant.
[0010] Preferably, in the aforementioned phosphogypsum-based grouting material for tunnel engineering, the special dispersant is composed of a mixture of one or two of A or B in any ratio, wherein, by weight, A consists of 65-70 parts of polycarboxylic acid water-reducing agent, 20-22 parts of polycarboxylic acid slump retaining agent, 0.1-0.2 parts of hydroxypropyl methylcellulose, 4-6 parts of sodium gluconate and 1-2 parts of sodium citrate; B consists of 55-65 parts of polycarboxylic acid water-reducing agent, 30-35 parts of polycarboxylic acid slump retaining agent, 0.1-0.2 parts of hydroxypropyl methylcellulose and 2-5 parts of modified aluminum hydroxide.
[0011] Preferably, in the aforementioned phosphogypsum-based grouting material for tunnel engineering, the polycarboxylic acid water-reducing agent has a water-reducing rate ≥ 25, the hydroxypropyl methylcellulose has a molecular weight of 6000, the sodium gluconate effective ingredient content ≥ 99%, the sodium citrate effective ingredient content ≥ 98%, and the modified aluminum hydroxide is a high-soluble aluminum hydroxide with an acid solubility rate > 95%.
[0012] Preferably, the phosphogypsum-based grouting material for the tunnel engineering is α-high-strength phosphogypsum, with an initial setting time of 2-6 min, a final setting time of 8-13 min, a 2h flexural strength of 4.5 MPa, and an absolute dry compressive strength of 49.8 MPa; the specific surface area of the sulphoaluminate cement is 360 m 2 / kg, initial setting time ≥25min, final setting time ≤180min, 3-day compressive strength ≥45MPa.
[0013] Preferably, in the aforementioned phosphogypsum-based grouting material for tunnel engineering, the limestone powder has a particle size of 180-200 mesh; the fly ash is Class I ash, with a water requirement of 99% and a loss on ignition of 0.2%.
[0014] Preferably, in the aforementioned phosphogypsum-based grouting material for tunnel engineering, the silica fume is non-densified silica fume with a particle size of 200-260 meshes.
[0015] Preferably, in the aforementioned phosphogypsum-based grouting material for tunnel engineering, the early strength agent is lithium carbonate or nano-silicon dioxide or a mixture of the two in any ratio.
[0016] The second technical solution of the present invention:
[0017] A method for preparing the aforementioned phosphogypsum-based grouting material for tunnel engineering comprises the following steps:
[0018] S1: By weight, 65-70 parts of polycarboxylate water reducer, 20-22 parts of polycarboxylate slump retainer, 0.1-0.2 parts of hydroxypropyl methylcellulose, 4-6 parts of sodium gluconate and 1-2 parts of sodium citrate are mixed evenly; or 55-65 parts of polycarboxylate water reducer, 30-35 parts of polycarboxylate slump retainer, 0.1-0.2 parts of hydroxypropyl methylcellulose and 2-5 parts of modified aluminum hydroxide are mixed evenly to prepare a special dispersant;
[0019] S2: Mix high-strength phosphogypsum and limestone powder evenly, then add sulphoaluminate cement, silica fume and fly ash, mix evenly, add early strength agent and special dispersant in sequence, and mix evenly again to obtain phosphogypsum-based grouting material for tunnel engineering; wherein, by weight, high-strength phosphogypsum is 40-50 parts, sulphoaluminate cement is 10-15 parts, fly ash is 5-7 parts, silica fume is 6-8 parts, limestone is 5-6 parts, early strength agent is 0.1-0.2 parts and special dispersant is 1-2 parts.
[0020] The third technical solution of the present invention:
[0021] An application of the aforementioned phosphogypsum-based grouting material in tunnel engineering, wherein the application method is to directly apply the grouting material after it is prepared according to the proportion and the method.
[0022] Beneficial effects of the present invention:
[0023] 1. The α high-strength phosphogypsum prepared in the present invention has an initial setting time of 2-8 min, a water-cement ratio of 0.30, and an absolute dry compressive strength of ≥45 MPa. At the same time, its hydration has a micro-expansion, which can improve the stone rate of the grouting material.
[0024] 2. The phosphogypsum-based grouting material of the present invention introduces limestone, and the Ca provided by the limestone 2+ SO4 with phosphogypsum 2- The reaction produces CaSO4, which promotes the hydration of phosphogypsum. At the same time, limestone is an alkaline substance that can neutralize the residual acid in phosphogypsum, adjust the pH value of phosphogypsum, and eliminate the influence of residual acid in phosphogypsum on its performance.
[0025] 3. The phosphogypsum-based grouting material of the present invention introduces non-densified silica fume and fly ash. The former mainly makes up for the defects of poor water resistance and easy water seepage of phosphogypsum, and the addition of the latter ensures the later strength of the grouting material.
[0026] 4. The phosphogypsum-based grouting material of the present invention can be widely used in tunnel seepage, water gushing and crack sealing, etc. It can effectively absorb industrial by-products, not only ensure the quality and safety of tunnel construction, but also promote waste recycling, contribute to clean production and sustainable development, and achieve "waste treatment with waste", which is in line with the requirements of green, orderly and low-carbon economic development.
[0027] 5. The special dispersant for phosphogypsum grouting material of the present invention can control the setting time of the grouting material by adjusting the dosage of the dispersant.
[0028] 6. The initial flow cone fluidity of the phosphogypsum grouting material prepared by the present invention is less than 30s, the 3h compressive strength is ≥3MPa, the 1d compressive strength is ≥12MPa, and the 28d compressive strength is ≥40MPa. DETAILED DESCRIPTION
[0029] The present invention will be further described below in conjunction with the embodiments, but they are not intended to limit the present invention.
[0030] Embodiments of the present invention
[0031] The raw material requirements used in the embodiments of the present invention are as follows:
[0032] The water reduction rate of polycarboxylate water reducer is ≥25;
[0033] The molecular weight of hydroxypropyl methylcellulose is 6000;
[0034] The active ingredient content of sodium gluconate is ≥99%;
[0035] The active ingredient content of sodium citrate is ≥98%;
[0036] Modified aluminum hydroxide is a highly soluble aluminum hydroxide with an acid solubility of more than 95%;
[0037] The high-strength phosphogypsum is α high-strength phosphogypsum, with an initial setting time of 2-6 minutes, a final setting time of 8-13 minutes, a 2-hour flexural strength of 4.5 MPa, and an absolute dry compressive strength of 49.8 MPa;
[0038] Sulphoaluminate cement specific surface area 360m 2 / kg, initial setting time ≥25min, final setting time ≤180min, 3-day compressive strength ≥45MPa;
[0039] The particle size of limestone powder is 180-200 mesh;
[0040] Fly ash is Class I ash, with a water requirement of 99% and a loss on ignition of 0.2%;
[0041] The silica fume is non-densified silica fume with a particle size of 200-260 mesh.
[0042] Example 1
[0043] A phosphogypsum-based grouting material for tunnel engineering consists, by weight, of 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of lithium carbonate early strength agent and 2 parts of special dispersant; wherein the special dispersant consists, by weight, of 68 parts of polycarboxylic acid water reducer, 21 parts of polycarboxylic acid slump retaining agent, 0.15 parts of hydroxypropyl methylcellulose, 5 parts of sodium gluconate and 1.5 parts of sodium citrate.
[0044] Example 2
[0045] A phosphogypsum-based grouting material for tunnel engineering comprises, by weight, 40 parts of high-strength phosphogypsum, 10 parts of sulphoaluminate cement, 5 parts of fly ash, 6 parts of silica fume, 5 parts of limestone, 0.1 parts of an early strength agent and 1 part of a special dispersant; wherein the special dispersant comprises, by weight, 65 parts of a polycarboxylic acid water-reducing agent, 20 parts of a polycarboxylic acid slump-retaining agent, 0.1 parts of hydroxypropyl methylcellulose, 4 parts of sodium gluconate and 1 part of sodium citrate.
[0046] Example 3
[0047] A phosphogypsum-based grouting material for tunnel engineering comprises, by weight, 50 parts of high-strength phosphogypsum, 15 parts of sulphoaluminate cement, 7 parts of fly ash, 8 parts of silica fume, 6 parts of limestone, 0.2 parts of an early strength agent and 2 parts of a special dispersant; wherein the special dispersant comprises, by weight, 70 parts of a polycarboxylic acid water reducer, 22 parts of a polycarboxylic acid slump retaining agent, 0.2 parts of hydroxypropyl methylcellulose, 6 parts of sodium gluconate and 2 parts of sodium citrate.
[0048] Example 4
[0049] A phosphogypsum-based grouting material for tunnel engineering consists, by weight, of 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of lithium carbonate early strength agent and 2 parts of special dispersant; wherein the special dispersant consists of A and B in a mass ratio of 1:1, and by weight, A consists of 68 parts of polycarboxylate water reducer, 21 parts of polycarboxylate slump retainer, 0.15 parts of hydroxypropyl methylcellulose, 5 parts of sodium gluconate and 1.5 parts of sodium citrate; and B consists of 60 parts of polycarboxylate water reducer, 32 parts of polycarboxylate slump retainer, 0.15 parts of hydroxypropyl methylcellulose and 4 parts of modified aluminum hydroxide.
[0050] Example 5
[0051] A phosphogypsum-based grouting material for tunnel engineering consists, by weight, of 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of lithium carbonate early strength agent and 2 parts of special dispersant; wherein the special dispersant consists of A and B in a mass ratio of 2:1, and by weight, A consists of 66 parts of polycarboxylate water reducer, 20 parts of polycarboxylate slump retainer, 0.1 part of hydroxypropyl methylcellulose, 4 parts of sodium gluconate and 1 part of sodium citrate; and B consists of 65 parts of polycarboxylate water reducer, 35 parts of polycarboxylate slump retainer, 0.2 parts of hydroxypropyl methylcellulose and 5 parts of modified aluminum hydroxide.
[0052] Example 6
[0053] A phosphogypsum-based grouting material for tunnel engineering consists, by weight, of 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of lithium carbonate early strength agent and 2 parts of special dispersant; wherein the special dispersant consists of A and B in a mass ratio of 1:2, and by weight, A consists of 70 parts of polycarboxylate water reducer, 22 parts of polycarboxylate slump retainer, 0.2 parts of hydroxypropyl methylcellulose, 6 parts of sodium gluconate and 2 parts of sodium citrate; and B consists of 55 parts of polycarboxylate water reducer, 30 parts of polycarboxylate slump retainer, 0.1 parts of hydroxypropyl methylcellulose and 2 parts of modified aluminum hydroxide.
[0054] Example 7
[0055] A method for preparing high-strength phosphogypsum comprises the following steps:
[0056] S1: Take a phosphoric acid solution with a mass concentration of 20%, heat it to 90°C, and obtain a hot phosphoric acid solution;
[0057] S2: Add dihydrate gypsum into hot phosphoric acid solution at a solid-liquid ratio of 1kg:2L, stir at 200r / min for 1h to obtain slurry;
[0058] S3: The slurry is filtered, and the solid matter is first washed with boiling water, then washed with anhydrous ethanol, and finally dried at 59°C to constant weight to obtain high-strength phosphogypsum.
[0059] Example 8
[0060] A method for preparing phosphogypsum-based grouting material for tunnel engineering, comprising the following steps:
[0061] S1: uniformly mix polycarboxylate water reducer, polycarboxylate slump retainer, hydroxypropyl methylcellulose, sodium gluconate and sodium citrate in proportion; or uniformly mix polycarboxylate water reducer, polycarboxylate slump retainer, hydroxypropyl methylcellulose and modified aluminum hydroxide in proportion to prepare a special dispersant; the two special dispersants can be used alone or in any proportion;
[0062] S2: Mix high-strength phosphogypsum and limestone powder evenly, then add sulphoaluminate cement, silica fume and fly ash, mix evenly, add early strength agent and special dispersant in sequence, and mix evenly again to obtain phosphogypsum-based grouting material for tunnel engineering.
[0063] Application examples:
[0064] According to the two formulas in Table 1, 4 groups of samples were prepared for each formula, and then special dispersants were added to the samples according to the ratio in Table 2 (wherein, by weight, A consists of 68 parts of polycarboxylate water reducer, 21 parts of polycarboxylate slump retainer, 0.15 parts of hydroxypropyl methylcellulose, 5 parts of sodium gluconate and 1.5 parts of sodium citrate; B consists of 60 parts of polycarboxylate water reducer, 32 parts of polycarboxylate slump retainer, 0.15 parts of hydroxypropyl methylcellulose and 4 parts of modified aluminum hydroxide), and the setting time, 3h strength / MPa, 1d strength / MPa and 28d strength / MPa were tested respectively. The results are shown in Table 2:
[0065] Table 1 Two different formulations
[0066] formula Alpha phosphogypsum Sulphoaluminate cement Silica Fume Fly ash Limestone powder Nano Silica 1 50% 18% 8% 20% 4% 0.1% of the total mass of the above ingredients 2 40% 20% 12% 25% 3% 0.1% of the total mass of the above ingredients
[0067] Table 2 Performance test results of different formulations
[0068]
[0069] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical solutions and inventive concepts of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A phosphogypsum-based grouting material for tunnel engineering, characterized in that: Calculated by weight, it includes 40-50 parts of high-strength phosphogypsum, 10-15 parts of sulphoaluminate cement, 5-7 parts of fly ash, 6-8 parts of silica fume, 5-6 parts of limestone, 0.1-0.2 parts of early strength agent and 1-2 parts of special dispersant.
2. The phosphogypsum-based grouting material for tunnel engineering according to claim 1, characterized in that: Calculated by weight, it includes 45 parts of high-strength phosphogypsum, 12 parts of sulphoaluminate cement, 6 parts of fly ash, 7 parts of silica fume, 6 parts of limestone, 0.2 parts of early strength agent and 2 parts of special dispersant.
3. The phosphogypsum-based grouting material for tunnel engineering according to claim 1 or 2, characterized in that: The special dispersant is composed of a mixture of one or two of A or B in any ratio, wherein, by weight, A consists of 65-70 parts of polycarboxylic acid water-reducing agent, 20-22 parts of polycarboxylic acid slump-retaining agent, 0.1-0.2 parts of hydroxypropyl methylcellulose, 4-6 parts of sodium gluconate and 1-2 parts of sodium citrate; and B consists of 55-65 parts of polycarboxylic acid water-reducing agent, 30-35 parts of polycarboxylic acid slump-retaining agent, 0.1-0.2 parts of hydroxypropyl methylcellulose and 2-5 parts of modified aluminum hydroxide.
4. The phosphogypsum-based grouting material for tunnel engineering according to claim 3, characterized in that: The water reduction rate of the polycarboxylate water reducer is ≥25, the molecular weight of hydroxypropyl methylcellulose is 6000, the effective component content of sodium gluconate is ≥99%, the effective component content of sodium citrate is ≥98%, and the modified aluminum hydroxide is a high-soluble aluminum hydroxide with an acid solubility rate of >95%.
5. The phosphogypsum-based grouting material for tunnel engineering according to claim 1 or 2, characterized in that: The high-strength phosphogypsum is α high-strength phosphogypsum, with an initial setting time of 2-6 minutes, a final setting time of 8-13 minutes, a 2-hour flexural strength of 4.5 MPa, and an absolute dry compressive strength of 49.8 MPa; the specific surface area of the sulphoaluminate cement is 360 m 2 / kg, initial setting time ≥25min, final setting time ≤180min, 3-day compressive strength ≥45MPa.
6. The phosphogypsum-based grouting material for tunnel engineering according to claim 1 or 2, characterized in that: The particle size of the limestone powder is 180-200 meshes; the fly ash is Class I ash, with a water requirement of 99% and a loss on ignition of 0.2%.
7. The phosphogypsum-based grouting material for tunnel engineering according to claim 1 or 2, characterized in that: The silica fume is non-densified silica fume with a particle size of 200-260 meshes.
8. The phosphogypsum-based grouting material for tunnel engineering according to claim 1 or 2, characterized in that: The early strength agent is one of lithium carbonate and nano silicon dioxide or a mixture of the two in any ratio.
9. A method for preparing the phosphogypsum-based grouting material for tunnel engineering according to any one of claims 1 to 8, characterized in that: The steps include: S1: uniformly mix polycarboxylate water reducer, polycarboxylate slump retainer, hydroxypropyl methylcellulose, sodium gluconate and sodium citrate in proportion; or uniformly mix polycarboxylate water reducer, polycarboxylate slump retainer, hydroxypropyl methylcellulose and modified aluminum hydroxide in proportion to prepare a special dispersant; S2: Mix high-strength phosphogypsum and limestone powder evenly, then add sulphoaluminate cement, silica fume and fly ash, mix evenly, add early strength agent and special dispersant in sequence, and mix evenly again to obtain phosphogypsum-based grouting material for tunnel engineering.
10. Use of the phosphogypsum-based grouting material according to any one of claims 1 to 8 in tunnel engineering.
Citation Information
Cited By
Sludge synergistic curing agent based on microbial mineralization and nano-compounding and preparation method of sludge synergistic curing agent
CN121020937A
A sludge synergistic stabilizer based on microbial mineralization and nanocomposite and a preparation method thereof
CN121020937B