Fly ash brick baking-free brick and preparation method thereof

By combining constant temperature pre-curing and microwave curing, the problems of long curing time and high energy consumption of fly ash bricks have been solved, realizing efficient and low-energy production of fly ash bricks, which is in line with the goal of green and low-carbon development.

CN118930217AInactive Publication Date: 2024-11-12CHINA UNIV OF GEOSCIENCES (BEIJING)
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411158906.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fly ash bricks have long curing times, high energy consumption, and complex processes, which do not meet the goals of green and low-carbon social development.

Method used

By combining constant temperature pre-curing and microwave curing, curing time is shortened, energy consumption is reduced, and production efficiency is improved.

Benefits of technology

It significantly reduces maintenance time, lowers energy consumption, and improves production efficiency. The process is simple, aligns with the goals of green and low-carbon social development, and possesses strong market competitiveness and environmental benefits.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a fly ash brick baking-free brick and a preparation method thereof, and belongs to the technical field of building material preparation, and the preparation method comprises the following steps: 1, carrying out pretreatment on fly ash and quartz sand; 2, preparing a solid-phase raw material; 3, preparing a liquid-phase raw material; step 4, compression molding; and fifthly, the demolded product is cured. According to the fly ash brick baking-free brick and the preparation method thereof, a constant-temperature pre-curing and microwave curing combined method is adopted, high-temperature long-time curing is not needed, the curing time is greatly shortened, the energy consumption is reduced, the production efficiency is improved, the technological process is simple, operation is convenient, and the development target of the green and low-carbon society is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material preparation, in particular to a fly ash unburned brick and a preparation method thereof. Background Art

[0002] Fly ash bricks are wall bricks made of fly ash and sand (or slag) through proportioning, mixing, molding and curing. Thermal curing is a necessary means for fly ash bricks to produce early strength. Generally, standard curing, autoclave curing, natural curing (watering) and water curing are used. Compared with traditional steam curing, microwave curing is essentially different in heating method and heat flow rate. It achieves synchronous heating of the whole sample through electromagnetic wave radiation, and has the characteristics of fast heating speed and uniform heating of the sample, saving energy consumption and curing time.

[0003] The patent number is 201610652788.3, ​​and the patent name is a fly ash and construction waste unfired brick and its preparation method. It reiterates that the fly ash unfired brick product is naturally cured for 2 to 4 hours after being formed and then demolded. The product enters a curing kiln with a temperature of 22 to 27°C and a relative humidity of 85 to 89% for curing for 60 to 80 hours. The curing cycle is relatively long and the process flow is more complicated than microwave curing. Summary of the invention

[0004] The purpose of the present invention is to provide a fly ash brick that does not require firing and a preparation method thereof. The method adopts a combination of constant temperature pre-curing and microwave curing, and does not require high temperature and long-term curing, which greatly reduces the curing time, reduces energy consumption, and improves production efficiency. The process flow is simple and easy to operate, which is in line with the development goals of a green and low-carbon society.

[0005] To achieve the above object, the present invention provides a method for preparing fly ash unburned bricks, comprising the following steps:

[0006] Step 1: Preliminary treatment of fly ash and quartz sand;

[0007] Step 2: preparing solid phase raw materials;

[0008] Step 3, preparing liquid raw materials;

[0009] Step 4: Pressing and forming;

[0010] Step 5: Maintain the demoulded products.

[0011] Preferably, the specific operation of step one is: feeding fly ash and quartz sand into a ball mill for fine grinding to 100-150 meshes.

[0012] Preferably, the specific operation of the step 2 is: mixing the treated fly ash and quartz sand obtained in the step 1 evenly to form a mixture, which is a solid raw material.

[0013] Preferably, the specific operation of step three is: mixing water glass and sodium hydroxide in a certain proportion and stirring evenly to obtain an alkali activator, that is, a liquid phase raw material, and the liquid phase modulus of the alkali activator is 1.25 to 1.45.

[0014] Preferably, the specific operation of step 4 is: uniformly mixing the solid-phase raw material and the liquid-phase raw material according to a certain mass ratio, and putting them into a mold for pressure molding.

[0015] Preferably, the curing in step five includes constant temperature curing or industrial microwave curing after constant temperature curing.

[0016] Preferably, in the solid raw material of step 2, the fly ash accounts for 70-75% by mass, and the quartz sand accounts for 25-30% by mass.

[0017] Preferably, in step 4, the mass ratio of the solid raw material to the liquid raw material is 3:1 to 3.4:1, and the pressurization pressure is 15 to 20 MPa.

[0018] Preferably, in the step 5, the curing temperature in the constant temperature curing box is 60° C., and the curing time is 6 to 8 hours, or the constant temperature curing temperature is 60° C., and the curing time is 2 to 4 hours, and the industrial microwave curing conditions are curing at 160 to 200 W for 20 to 25 minutes.

[0019] The present invention also provides a fly ash unburned brick prepared by the preparation method.

[0020] Therefore, the present invention adopts the above-mentioned fly ash brick unburned brick and preparation method thereof, which has the following beneficial effects:

[0021] (1) The method of combining constant temperature pre-curing and microwave curing is adopted, which eliminates the need for high temperature and long-term curing, greatly reduces the curing time, reduces energy consumption, and improves production efficiency. The process is simple and easy to operate, which is in line with the development goals of a green and low-carbon society.

[0022] (2) By improving the preparation method to reduce the curing time and curing temperature, the use of fly ash and other materials to prepare environmentally friendly bricks is more economical, has better market competitiveness and good market prospects, and can effectively turn waste slag into resources, achieving a virtuous cycle of emission and utilization. It is one of the most effective and thorough ways to eliminate industrial waste pollution.

[0023] The technical solution of the present invention is further described in detail below through embodiments. DETAILED DESCRIPTION

[0024] The technical solution of the present invention is further illustrated by the following embodiments.

[0025] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0026] Example

[0027] The present invention provides a method for preparing fly ash unburned bricks, comprising the following steps:

[0028] Step 1: Preliminary treatment of fly ash and quartz sand;

[0029] The fly ash and quartz sand are sent to the ball mill for fine grinding to 100-150 mesh. The use of fly ash to make bricks reduces the dependence on natural clay resources and helps to protect farmland. The reuse of fly ash avoids the environmental pollution caused by its discharge as waste.

[0030] Quartz sand is hard and wear-resistant. When added as aggregate to unfired bricks, it can provide the necessary mechanical strength and durability and enhance the structural stability of the bricks. Quartz sand has stable chemical properties and is resistant to acid and alkali corrosion, which is conducive to the long-term stability of brick performance. In the preparation process of unfired bricks, fly ash and quartz sand not only play the advantages of environmental protection and energy saving, but also ensure the physical properties and economy of bricks. They are an important part of the development of green building materials.

[0031] Step 2: preparing solid phase raw materials;

[0032] The treated fly ash and quartz sand obtained in step 1 are mixed evenly to form a mixture, which is a solid raw material, wherein the fly ash accounts for 70-75% by mass and the quartz sand accounts for 25-30% by mass.

[0033] Step 3, preparing liquid raw materials;

[0034] The water glass and sodium hydroxide are mixed in a certain proportion and stirred evenly to obtain an alkali activator, which is a liquid phase raw material. The liquid phase modulus of the alkali activator is 1.25-1.45.

[0035] As a strong alkali, sodium hydroxide can accelerate the hydrolysis reaction of water glass and promote the rapid formation of silicate gel, thereby shortening the production cycle and improving production efficiency.

[0036] Water glass can undergo hydrolysis when it encounters water or under certain alkaline conditions to generate silica gel with gelling properties. This gel can bond aggregates such as fly ash and quartz sand together to form a solid whole, replacing the ceramic bonding in the traditional sintering process. The formation of silicate gel enhances the compressive and flexural strength of bricks, allowing unfired bricks to meet certain mechanical performance requirements even without high-temperature firing.

[0037] Step 4: Pressing and forming;

[0038] The solid raw material and the liquid raw material are uniformly mixed in a mass ratio of 3:1 to 3.4:1, and the mixture is put into a mold and pressurized at 15 to 20 MPa to form the mixture.

[0039] Step 5: Microwave curing;

[0040] The product demoulded after molding in step 4 is cured in a constant temperature curing box at 60°C for 6 to 8 hours, or cured in a constant temperature curing box at 60°C for 2 to 4 hours and then cured for 20 to 25 minutes using industrial microwaves at 160 to 200W to obtain fly ash unburned bricks. Fly ash and quartz are used as solid raw materials, alkali activator is used as liquid phase, and microwave curing method is used to prepare fly ash bricks, which improves the diversification of fly ash utilization process, shortens curing time, reduces energy consumption, and improves fly ash utilization efficiency.

[0041] After the sample is pressure-formed, it is cured at a constant temperature of 60°C for 2 to 4 hours, and then cured at 160W to 200W using industrial microwaves for 20 to 25 minutes. This preparation method improves production efficiency and greatly shortens the curing time. The fly ash unburned bricks obtained have the following properties:

[0042] Table 1 Technical performance of fly ash unburned bricks

[0043] project Product performance <![CDATA[Bulk density (g / cm 3 )]]> 1.71~1.78 <![CDATA[Water content (w B %)]]> 2.36~2.7 Water absorption (%) 11.73~11.44 Acid leaching loss rate (%) 2.04~4.22 7d saturated flexural strength / MPa 5.76~6.93 7d saturated flexural strength / MPa 25.65~27.56 Thermal conductivity (W / m·k) 0.383~0.385 Linear expansion coefficient (25℃~100℃) <![CDATA[9.61×10 -6 ]]> Volume expansion (25℃~100℃) <![CDATA[237.72×10 -7 ]]> Flexural strength after 10 thermal shock cycles / MPa 4.53~5.85 Compressive strength after 100 freeze-thaw cycles / MPa 20.08~22.32

[0044] The data shows that the product performance meets the MU25 standard requirements of "JC / T239-2014 Autoclaved Fly Ash Bricks". The 7d saturated flexural strength of the sample reaches 5.76~6.93MPa, which is greater than the 4.5MPa required in the standard, and the compressive strength is 25.65~27.56MPa, which is higher than the 25MPa required in the standard.

[0045] Embodiment 1

[0046] A method of preparing fly ash unburned bricks using fly ash, wherein the main raw material fly ash comes from fly ash in power plants, quartz sand comes from sand and gravel for construction, and alkali activator comes from sodium hydroxide and water glass, and the modulus of the alkali activator after mixing is 1.25. The dosage of each component is: 70 parts of fly ash, 30 parts of quartz sand, and 30 parts of alkali activator.

[0047] The specific method of the present invention for preparing fly ash brick without burning by utilizing fly ash is as follows: fly ash and quartz sand are respectively put into a ball mill and finely ground to 150 mesh, then the solid and liquid raw materials are mixed and stirred evenly according to the above proportion, put into a mold and pressurized to 15Mpa for molding, and after demolding, the product is put into a constant temperature curing box at 60°C for curing for 6 hours, and the average saturated compressive strength of the product at 7d is measured to be 28.50MPa, and the average flexural strength is 6.90MPa.

[0048] Embodiment 2

[0049] A method of preparing fly ash unburned bricks using fly ash, wherein the main raw material fly ash comes from fly ash from power plants, quartz sand comes from sand and gravel for construction, and alkali activator comes from sodium hydroxide and water glass, and the modulus of the alkali activator after mixing is 1.45. The dosage of each component is: 75 parts of fly ash, 25 parts of quartz sand, and 34 parts of alkali activator.

[0050] The specific method of the present invention for preparing fly ash brick without firing by utilizing fly ash is as follows: fly ash and quartz sand are respectively put into a ball mill and finely ground to 100 mesh, then the solid and liquid raw materials are mixed and stirred evenly according to the above proportion, put into a mold and pressurized to 20Mpa for molding, and after demolding, the product is put into a constant temperature curing box and cured at 60°C for 8h, and the average saturated compressive strength of the product at 7d is measured to be 30.50MPa, and the average flexural strength is 8.84MPa.

[0051] Embodiment 3

[0052] A method of preparing fly ash unburned bricks using fly ash, wherein the main raw material fly ash comes from fly ash in power plants, quartz sand comes from sand and gravel for construction, and alkali activator comes from sodium hydroxide and water glass, and the modulus of the alkali activator after mixing is 1.25. The dosage of each component is: 70 parts of fly ash, 30 parts of quartz sand, and 30 parts of alkali activator.

[0053] The specific method of the present invention for preparing fly ash brick without burning by utilizing fly ash is as follows: fly ash and quartz sand are respectively put into a ball mill and finely ground to 100 mesh, then the solid and liquid raw materials are mixed and stirred evenly according to the above proportion, put into a mold and pressurized to 15Mpa for molding, after demolding, the product is put into a constant temperature curing box for curing at 60°C for 2h, and then put into an industrial microwave equipment for curing at 200W for 20min, and the average saturated compressive strength of the product at 7d is measured to be 25.12MPa, and the average flexural strength is 5.81MPa.

[0054] Embodiment 4

[0055] A method of preparing fly ash unburned bricks using fly ash, wherein the main raw material fly ash comes from fly ash in power plants, quartz sand comes from sand and gravel for construction, and alkali activator comes from sodium hydroxide and water glass, and the modulus of the alkali activator after mixing is 1.35. The dosage of each component is: 73 parts of fly ash, 27 parts of quartz sand, and 32 parts of alkali activator.

[0056] The specific method of the present invention for preparing fly ash brick without burning by utilizing fly ash is as follows: fly ash and quartz sand are respectively put into a ball mill and finely ground to 100 mesh, then the solid and liquid raw materials are mixed and stirred evenly according to the above proportion, put into a mold and pressurized to 20Mpa for molding, after demolding, the product is put into a constant temperature curing box for curing at 60°C for 3h, and then put into an industrial microwave equipment for curing at 160W for 25min, and the average saturated compressive strength of the product at 7d is measured to be 25.63MPa, and the average flexural strength is 5.96MPa.

[0057] Embodiment 5

[0058] A method of preparing fly ash unburned bricks using fly ash, wherein the main raw material fly ash comes from fly ash from power plants, quartz sand comes from sand and gravel for construction, and alkali activator comes from sodium hydroxide and water glass, and the modulus of the alkali activator after mixing is 1.45. The dosage of each component is: 75 parts of fly ash, 25 parts of quartz sand, and 34 parts of alkali activator.

[0059] The specific method of the present invention for preparing fly ash brick without burning by utilizing fly ash is as follows: fly ash and quartz sand are respectively put into a ball mill and finely ground to 100 mesh, then the solid and liquid raw materials are mixed and stirred evenly according to the above proportion, put into a mold and pressurized to 20Mpa for molding, after demolding, the product is put into a constant temperature curing box for curing at 60°C for 4h, and then put into an industrial microwave equipment for curing at 180W for 22min, and the average saturated compressive strength of the product at 7d is measured to be 26.23MPa, and the average flexural strength is 6.62MPa.

[0060] Therefore, the present invention adopts the above-mentioned fly ash brick unburned brick and its preparation method, and adopts a method combining constant temperature pre-curing and microwave curing. It does not require high temperature and long-term curing, which greatly reduces the curing time, reduces energy consumption, and improves production efficiency. The process flow is simple and easy to operate, which is in line with the development goals of a green and low-carbon society.

[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A method for preparing fly ash unfired bricks, characterized in that: The following steps are involved: Step 1: Preliminary treatment of fly ash and quartz sand; Step 2: preparing solid phase raw materials; Step 3, preparing liquid raw materials; Step 4: Pressing and forming; Step 5: Maintain the demoulded products.

2. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: The specific operation of step 1 is: sending fly ash and quartz sand into a ball mill for fine grinding to 100-150 meshes.

3. The method for preparing a fly ash unburned brick according to claim 1, characterized in that: The specific operation of the step 2 is: mixing the treated fly ash and quartz sand obtained in the step 1 evenly to form a mixture, which is the solid raw material.

4. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: The specific operation of step three is: mixing water glass and sodium hydroxide in a certain proportion and stirring evenly to obtain an alkali activator, which is a liquid phase raw material, and the liquid phase modulus of the alkali activator is 1.25-1.

45.

5. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: The specific operation of step 4 is: mixing the solid raw material and the liquid raw material evenly according to a certain mass ratio, putting them into a mold and pressurizing them.

6. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: The curing in step 5 includes one of constant temperature curing or industrial microwave curing after constant temperature curing.

7. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: In the step 2, the fly ash in the solid raw material accounts for 70-75% by mass, and the quartz sand accounts for 25-30% by mass.

8. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: In the step 4, the mass ratio of the solid raw material to the liquid raw material is 3:1 to 3.4:1, and the pressurization pressure is 15 to 20 MPa.

9. The method for preparing fly ash unburned bricks according to claim 1, characterized in that: In the step 5, the curing temperature in the constant temperature curing box is 60° C., and the curing time is 6 to 8 hours, or the constant temperature curing temperature is 60° C., and the curing time is 2 to 4 hours, and the industrial microwave curing condition is curing at 160 to 200W for 20 to 25 minutes.

10. A fly ash brick without burning, characterized in that: The fly ash unburned brick is prepared by the preparation method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing high-strength mortar and concrete by using low-quality fly ash

    CN108751917A

  • Production method of baking-free brick by utilizing industrial tailings and coal ash

    CN109206116A

  • ECO- efficient geopolymer bricks

    IN202141004597A

  • Alkall-activated masonry products with no cement

    KR1020110000441A

  • Fly ash-containing construction material with improved strength and water resistance and methods of forming the same

    US20180312438A1