Preparation method of high-performance aluminum oxide composite ceramic
Through casting and sintering technology, the mechanical and electrical properties of the alumina electrostatic chuck was solved. Through powder pretreatment and sol molding, combined with PVB resin and dispersant, a uniform slurry was formed, and presintering and heating were used. Pressure sintering method improves the densification degree of ceramics and achieves efficient mass production and excellent performance electrostatic chuck dielectric ceramics.
Patent Information
- Application Number
- CN202410864457.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing alumina electrostatic chucks have shortcomings in terms of mechanical properties, electrical properties and thermal shock resistance, and the dispersion of nano silicon carbide and difficulty in sintering and densification affects their service life and performance.
Cast molding and sintering technology is adopted, and powder pretreatment and sol molding are combined with PVB resin and dispersant to form a uniform slurry, vacuum defoaming and casting are carried out, and presintering and hot pressing sintering are used to improve the The degree of densification and properties of ceramics.
Improve the mechanical properties and electrical properties of alumina composite ceramics, enhance the stability and durability of electrostatic chucks, solve the densification problems in sintering technology, and realize efficient mass production and excellent performance electrostatic chuck dielectric layer ceramics.
Smart Images

Figure CN118930230A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparation of electrostatic chuck ceramic plates, and in particular to a preparation method of high-performance alumina composite ceramics. Background Art
[0002] In the semiconductor industry, precision ceramic parts play an important role in a series of processing links such as chemical vapor deposition, physical vapor deposition, ion implantation, and etching. Precision ceramic parts are usually prepared by molding and precision machining of materials such as aluminum oxide, aluminum nitride, silicon nitride, silicon carbide, and yttrium oxide, and have excellent properties such as high strength, corrosion resistance, and high precision. The electrostatic chuck device is a kind of precision ceramic part that has extremely high requirements for the ceramic dielectric layer. During the semiconductor manufacturing process, the electrostatic chuck can evenly fix the wafer on the sample table and maintain the uniform temperature of the wafer, which is convenient for the processing and production of the wafer. How to prepare a precision electrostatic chuck ceramic dielectric layer that meets the excellent mechanical properties, electrical properties, and long-term stable use required for semiconductor processing has always been the goal of many researchers.
[0003] Alumina electrostatic chuck is a widely used semiconductor precision device, and it has some defects since its development. The main defects are: the ceramic products obtained by dry pressing or casting, intermediate process processing and debinding sintering of ordinary alumina powder have the following problems: (a) Compared with SiC and Si3N4, the fracture toughness and fracture strength of Al2O3 ceramics are relatively low, and its strength decreases significantly at high temperatures, and there is also a problem of relatively weak thermal shock resistance; (b) The raw material purity is not enough, and the electrical properties of the prepared electrostatic chuck dielectric layer are weak, resulting in large dielectric loss and easy breakdown during use, and low service life; (c) During the wafer processing process, due to the defects of the surface ceramic dielectric layer, the local adsorption force of the electrostatic chuck is uneven or deteriorated, which can easily lead to wafer scrapping. (d) Under more complex processing conditions, the dielectric layer ceramic needs to have higher dielectric strength, lower dielectric loss and withstand voltage to prevent the ceramic from being broken down during use.
[0004] In recent years, the preparation technology of nanocomposite ceramics has attracted the attention of many scholars. The mechanical, electrical, magnetic, optical, thermal and other properties of different components in the composite material can be coupled or induced by each other. The composite material can obtain better performance than a single component or properties that a single component does not have. The composite effect is greater than the simple addition effect. Al2O3 / SiC composite ceramics have attracted much attention due to their excellent mechanical, thermal and electrical properties.
[0005] In terms of mechanical properties, the pinning effect of silicon carbide particles improves the fracture strength and fracture toughness of composite ceramics. Niihara's study on Al2O3 / SiC nanocomposites found that by adding 5vol% nano-SiC particles, the three-point bending strength increased from 320MPa of a single Al2O3 to 1050MPa of a nanocomposite. In terms of thermal behavior and electrical conductivity, Parchoviansky et al. studied the effect of SiC nanoparticle addition on the electrical conductivity and thermal conductivity of Al2O3 / SiC micro-nanocomposites at room temperature and high temperature. Different samples with SiC volume fractions ranging from 3vol% to 20vol% were prepared by hot pressing at 1740℃ and 30MPa pressure in an argon atmosphere. The results show that the thermal properties (thermal diffusivity and thermal conductivity) of Al2O3 / SiC nanocomposites are not affected by the size and shape of SiC particles, but by the volume content of these particles. Thermal conductivity increases with the content of SiC nanoparticles, increasing up to 35% (from 28 to 38 W / m K) when the volume fraction of these nanoparticles is 20 vol%. Regarding electrical conductivity, Parchoviansky et al. showed that the electrical conductivity increases with the content of SiC nanoparticles, especially in composites with a SiC volume fraction greater than or equal to 10 vol%. The results showed that at low SiC contents, the SiC particles could not connect to each other to form a continuous conductive network, a result confirmed by the increase in conductivity from 10-5 S / m (5 vol%) to 10-3 S / m (10 vol%) when the SiC content was greater than 10%. The same trend has been confirmed by other studies, such as the study by Sawaguchi et al. or Stauffer and Aharony, who proposed the addition of 17 vol% of a second phase to create an effective conductive path based on a mathematical model.
[0006] Silicon carbide mainly includes β-SiC and α-SiC. The Mohs hardness of β-SiC is 9.25-9.6, second only to diamond. β-SiC has high mechanical strength, wear resistance, corrosion resistance, high temperature resistance, creep resistance and fracture resistance. The sintering activity of β-SiC is better than that of α-SiC, and it has high thermal conductivity and low thermal expansion coefficient, which makes it have good thermal shock resistance. The typical microstructure nanocomposite material of Al2O3 / SiC consists of a polycrystalline alumina matrix with an average grain size of 1 to 5 μm and silicon carbide particles with a size of tens to hundreds of nanometers, which exist inside the matrix grains or on the grain boundaries. CN108495829B reports the effect of adding different volume fractions of β-silicon carbide and α-silicon carbide to alumina on electrostatic chuck, strength, thermal conductivity and withstand voltage. β-SiC can improve the durability of the electrostatic chuck. When the composite sintered body contains more αSiC, the conductivity of αSiC is lower than that of βSiC. Therefore, it is believed that the local heat generation when a small current flows through the sintered body becomes larger and the insulation breakdown is easy to occur. In addition, when the composite sintered body contains more αSiC, the charge is easily accumulated in the composite sintered body through plasma irradiation, and it becomes easy to discharge. As a result, the electrostatic chuck is damaged with the discharge. Although the mechanical and electrical properties of Al2O3 / SiC nanocomposites have been greatly improved, these advantages depend to a large extent on the dispersion of the second phase and the degree of densification of ceramic sintering. The volume fraction of nano-SiC particles is limited by the following factors: a. The ability of molding processing technology to make the particles evenly distributed; b. And the densification limit of the existing sintering method. Specifically, (a) the uniform dispersion of the second phase is crucial for the nanocomposite material to obtain better performance than the overall material; (b) nano-SiC is more active during sintering and is easy to decompose and disappear from the system. How to control the sintering conditions to regulate the structure is also a technical difficulty.
[0007] What kind of molding and sintering methods can effectively compound alumina and silicon carbide to obtain precision ceramics with desired properties is a technical problem that needs to be solved urgently. Summary of the invention
[0008] The technical problem to be solved by the present invention is to provide a method for preparing high-performance alumina composite ceramics to solve the problems raised in the background technology. Tape casting, due to its advantages of high uniformity, thin layer preparation capability, high precision, suitability for mass production, and high material utilization, is beneficial to improving the mechanical properties, electrical properties and stability of the electrostatic chuck.
[0009] In order to solve the above technical problems, the technical solution of the present invention is:
[0010] A method for preparing a high-performance alumina composite ceramic, the method comprising:
[0011] Powder pretreatment: Process the nano silicon carbide powder and then pre-disperse it in a horizontal ball mill, add a dispersant to destroy the hard agglomerates and soft agglomerates in the powder to make it dispersed evenly, and disperse the nano alumina powder;
[0012] The treated powder needs to be tested for the content of other substances. Among other substances, the content of surface metal impurities is less than 100ppm;
[0013] The content of silicon carbide in the powder pretreatment is 0-10wt%, and the content of aluminum oxide is 90-100wt%;
[0014] Sol: First add 0-60 parts of toluene, 0-20 parts of isopropanol and 1-5 parts of plasticizer into a pneumatic sol machine, slowly and evenly stir for 5-20 minutes, then slowly add 30-50 parts of PVB resin powder in small amounts several times, stir at high speed for 2-4 hours to ensure that the PVB resin powder is evenly and fully dissolved to form PVB colloid;
[0015] Dispersion: First weigh a certain amount of balls, toluene and n-butanol mixed solvent into a stirred mill, with the ratio of toluene to n-butanol being 3:1 to 1:1, then add the pretreated nano-silicon carbide and nano-alumina powders and additives in sequence, turn on the stirring switch and stir for 1 to 4 hours;
[0016] Mixing: Transfer the alumina and silicon carbide slurry in the stirred mill to the drum ball mill, add a certain amount of PVB colloid according to the formula, and run at a certain stirring rate for 24 hours;
[0017] Vacuum degassing: The slurry in the drum ball mill is sent into the degassing tank with N2 gas pressure, the viscosity of the slurry and the corresponding ambient temperature are measured, the water bath temperature is set according to the slurry viscosity and temperature, and the appropriate degassing vacuum degree and time are set. After the slurry is effectively degassed, it is aged for a period of time for use;
[0018] Molding and sintering: Set the scraper blade height to 0.3-0.6mm, the casting speed to 0-300mm / min, set the temperature and inlet and outlet air flux according to the environment, and set the temperature of the drying zone of the casting machine to 0-100℃. According to the type of silicon carbide powder, the slurry is cast to obtain gray-black, gray-white or green cast green billets through casting, and then cut, punch, print, laminate and isostatically press to obtain block green billets for secondary molding, and finally debinding and sintering.
[0019] Preferably, the nano silicon carbide powder is α-SiC or β-SiC, and the particle size of the α-SiC or β-SiC is 60nm-400nm, wherein the particle size D50=100-200nm, D10=30-50nm, D90=150-200nm, and D90 / D10=3-6.
[0020] Preferably, in the forming and sintering steps, the sintering is vacuum sintering or hot pressing sintering or isostatic pressing sintering under an argon protective atmosphere.
[0021] Preferably, the sintering is hot pressing sintering under argon protective atmosphere, the sintering temperature is 1500℃~1850℃, the sintering pressure is 20~50Mpa, the pressure is maintained for 1~2h, and then cooled to room temperature. Pre-sintering is performed before sintering, and the pre-sintering temperature is 550℃~600℃.
[0022] Preferably, the plasticizer is dibutyl phthalate, di-n-octyl phthalate or butyl benzyl phthalate, and the content of the plasticizer is 0-8wt%.
[0023] Preferably, the dispersant is PEG or fish oil or lecithin or oleic acid or oleic acid amide, and the content of the dispersant is 0-5wt%.
[0024] Preferably, the alumina powder is nano high-purity alumina powder, γ or α phase spherical particles, with a purity greater than or equal to 99.99%, a particle size D50=100-400nm, and BET=5-30m2 / g.
[0025] Preferably, the α-SiC or β-SiC is nanometer high-purity silicon carbide, which is spherical particles of α phase or β phase or both, with a purity greater than or equal to 99.99%, the appearance color of silicon carbide is black, green or grayish white, the particle size D50 = 50 ~ 300nm, BET = 6 ~ 38m2 / g, and the volume fraction of silicon carbide accounts for 0 ~ 20% of the total.
[0026] The above technical solution has the following beneficial effects:
[0027] The present invention prepares nano-alumina and silicon carbide by tape casting and sintering; (1) nano-powders are difficult to form by ordinary molding methods due to their small particle size and large specific surface area, and excessive organic matter content in the organic solvent system is not conducive to molding. By optimizing material selection and process treatment in the early stage, a slurry system for stable tape casting is created. Through tape casting, composite ceramics can be formed in batches, greatly improving production efficiency; (2) Based on theory and reality, through treatment, alumina / silicon carbide is easier to disperse in the organic system, and electrostatic chuck dielectric layer ceramics with excellent mechanical and electrical properties are prepared; (3) The product obtained by tape casting has good uniformity and adjustable thickness, which is convenient for macroscopically regulating the microstructure of the electrostatic chuck; (4) In view of the difficulty in densification of multi-phase ceramics, a pre-sintering-HIP consolidation method is adopted to further improve the volume density of nano-composite ceramics and solve the technical problem of sintering Al2O3 / SiC ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a green body image of the Al2O3 / SiC composite ceramic obtained by tape casting of the present invention;
[0029] Figure 2 XRD spectrum of the Al2O3 / SiC composite ceramic of the present invention;
[0030] Figure 3 Schematic diagram of the microstructure of Al2O3 / SiC composite ceramic prepared in the present invention. DETAILED DESCRIPTION
[0031] The specific embodiments of the present invention are further described below in conjunction with the accompanying drawings. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0032] Example 1
[0033] A method for preparing a high-performance alumina composite ceramic, the preparation method comprising:
[0034] Powder pretreatment: Process the nano silicon carbide powder and then pre-disperse it in a horizontal ball mill, add a dispersant to destroy the hard agglomerates and soft agglomerates in the powder to make it dispersed evenly, and disperse the nano alumina powder;
[0035] The nano silicon carbide powder is α-SiC, the particle size of α-SiC is 60nm, wherein the particle size D50=100nm, D10=3nm, D90=200nm, and D90 / D10=3;
[0036] In other implementations of this embodiment, the particle size of α-SiC is 400 nm, wherein the particle size D50=200 nm, D10=50 nm, D90=200 nm, and D90 / D10=6;
[0037] α-SiC nanometer high-purity silicon carbide is a spherical particle of α phase, with a purity greater than or equal to 99.99%, the appearance color of silicon carbide is black, green or grayish white, the particle size D50 = 50nm, BET = 6m2 / g, and the volume fraction of silicon carbide accounts for 0% of the total. In other embodiments of this embodiment, the particle size D50 = 300nm, BET = 38m2 / g, and the volume fraction of silicon carbide accounts for 20% of the total.
[0038] The alumina powder is nano high-purity alumina powder, γ-phase spherical particles, with a purity greater than or equal to 99.99%, a particle size D50 = 100 nm, and BET = 5 m2 / g. In other embodiments of this embodiment, the particle size D50 = 400 nm, and BET = 30 m2 / g;
[0039] The treated powder needs to be tested for the content of other substances. Among other substances, the content of surface metal impurities is less than 100ppm;
[0040] The content of silicon carbide in the powder pretreatment accounts for 0wt%, and the content of aluminum oxide accounts for 100wt%. In other embodiments of this embodiment, the content of silicon carbide in the pretreatment accounts for 10wt%, and the content of aluminum oxide accounts for 90wt%;
[0041] Sol: first add 0 parts of toluene, 0 parts of isopropanol and 1 part of plasticizer into a pneumatic sol machine, stir slowly and evenly for 5 minutes, then slowly add 30 parts of PVB resin powder in small amounts at multiple times, stir at high speed for 2 hours, ensure that the PVB resin powder is evenly and fully dissolved to form a PVB colloid. In other embodiments of this embodiment, add 60 parts of toluene, 20 parts of isopropanol and 5 parts of plasticizer into a pneumatic sol machine, stir slowly and evenly for 20 minutes, then slowly add 50 parts of PVB resin powder in small amounts at multiple times, stir at high speed for 4 hours, ensure that the PVB resin powder is evenly and fully dissolved to form a PVB colloid;
[0042] The plasticizer is dibutyl phthalate, di-n-octyl phthalate, or butyl benzyl phthalate, and the content of the plasticizer is 0wt%. In other embodiments of this embodiment, the content of the plasticizer is 8wt%;
[0043] Dispersion: First weigh a certain amount of balls, toluene and n-butanol mixed solvent into a stirred mill, with the ratio of toluene to n-butanol being 3:1, then add the pretreated nano-silicon carbide and nano-alumina powder dispersants and additives in sequence, turn on the stirring switch and stir for 1 hour;
[0044] The dispersant is PEG or fish oil or lecithin or oleic acid or oleic acid amide, and the content of the dispersant is 0wt%. In other embodiments of this embodiment, the content of the dispersant is 5wt%;
[0045] Mixing: Transfer the alumina and silicon carbide slurry in the stirred mill to the drum ball mill, add a certain amount of PVB colloid according to the formula, and run at a certain stirring rate for 24 hours;
[0046] Vacuum degassing: The slurry in the drum ball mill is sent into the degassing tank with N2 gas pressure, the viscosity of the slurry and the corresponding ambient temperature are measured, the water bath temperature is set according to the slurry viscosity and temperature, and the appropriate degassing vacuum degree and time are set. After the slurry is effectively degassed, it is aged for a period of time for use;
[0047] Molding and sintering: The scraper blade height is set to 0.3mm, the casting speed is 0-300mm / min, and in other embodiments of the present embodiment, the casting speed is 150mm / min. The temperature of the drying zone of the casting machine is set at 0-100°C according to the environment setting temperature and the inlet and outlet air flux. In other embodiments of the present embodiment, the temperature of the drying zone of the casting machine is set at 80°C. According to the type of silicon carbide powder, the slurry is formed by casting to obtain gray-black, gray-white or green cast green billets, and then cut, punched, printed, laminated and isostatically pressed to obtain block green billets. Finally, the binder is removed and sintered. The sintering is vacuum sintering or hot pressing sintering under argon protective atmosphere or isostatic pressing sintering. The sintering is hot pressing sintering under argon protective atmosphere. The sintering temperature is 1500°C, the sintering pressure is 20Mpa, the pressure is maintained for 1h, and then cooled to room temperature. Pre-sintering is performed before sintering, and the pre-sintering temperature is 550°C.
[0048] Example 2
[0049] A method for preparing a high-performance alumina composite ceramic, the preparation method comprising:
[0050] Powder pretreatment: Process the nano silicon carbide powder and then pre-disperse it in a horizontal ball mill, add a dispersant to destroy the hard agglomerates and soft agglomerates in the powder to make it dispersed evenly, and disperse the nano alumina powder;
[0051] The nano silicon carbide powder is β-SiC, the particle size of β-SiC is 200nm, wherein the particle size D50=150nm, D10=40nm, D90=170nm, D90 / D10=5. In other implementations of this embodiment, the nano silicon carbide powder is a mixture of α-SiC and β-SiC;
[0052] β-SiC is nanometer high-purity silicon carbide, which is a spherical particle of β phase, with a purity greater than or equal to 99.99%, and the appearance color of silicon carbide is black, green or grayish white, with a particle size D50=300nm, BET=38m2 / g, and the volume fraction of silicon carbide accounts for 20% of the total. In other implementations of this embodiment, the particle size of silicon carbide is D50=200nm, BET=20m2 / g, and the volume fraction of silicon carbide accounts for 10% of the total;
[0053] The alumina powder is nano high-purity alumina powder, α-phase spherical particles, with a purity greater than or equal to 99.99%, a particle size D50 = 400nm, and BET = 30m2 / g;
[0054] The treated powder needs to be tested for the content of other substances. Among other substances, the content of surface metal impurities is less than 100ppm;
[0055] The content of silicon carbide in the powder pretreatment is 0-10wt%, and the content of aluminum oxide is 90-100wt%;
[0056] Sol: First add 30 parts of toluene, 10 parts of isopropanol and 3 parts of plasticizer into a pneumatic sol machine, slowly and evenly stir for 10 minutes, then slowly add 40 parts of PVB resin powder in small amounts several times, stir at high speed for 3 hours to ensure that the PVB resin powder is evenly and fully dissolved to form PVB colloid;
[0057] The plasticizer is dibutyl phthalate, di-n-octyl phthalate or butyl benzyl phthalate, and the content of the plasticizer is 4wt%;
[0058] Dispersion: First weigh a certain amount of balls, toluene and n-butanol mixed solvent into a stirred mill, with the ratio of toluene to n-butanol being 1:1, then add the pretreated nano-silicon carbide and nano-alumina powder dispersants and additives in sequence, turn on the stirring switch and stir for 4 hours;
[0059] The dispersant is PEG or fish oil or lecithin or oleic acid or oleic acid amide, and the content of the dispersant is 1wt%;
[0060] Mixing: Transfer the alumina and silicon carbide slurry in the stirred mill to the drum ball mill, add a certain amount of PVB colloid according to the formula, and run at a certain stirring rate for 24 hours;
[0061] Vacuum degassing: The slurry in the drum ball mill is sent into the degassing tank with N2 gas pressure, the viscosity of the slurry and the corresponding ambient temperature are measured, the water bath temperature is set according to the slurry viscosity and temperature, and the appropriate degassing vacuum degree and time are set. After the slurry is effectively degassed, it is aged for a period of time for use;
[0062] Molding and sintering: the scraper blade height is set to 0.3-0.6 mm, the casting speed is 0-300 mm / min, the temperature and the inlet and outlet air flux are set according to the environment, the temperature of the drying zone of the casting machine is set at 0-100°C, and according to the type of silicon carbide powder, the slurry is cast to obtain gray-black, gray-white or green cast green body after tape casting, and then cut, punched, printed, laminated and isostatically pressed to obtain block green body after secondary molding, and finally debinding and sintering, the sintering is vacuum sintering or hot pressing sintering under argon protective atmosphere or isostatic pressing sintering, the sintering is hot pressing sintering under argon protective atmosphere, the sintering temperature is 1850°C, the sintering pressure is 50Mpa, the pressure is maintained for 2 hours, and then cooled to room temperature, and pre-sintering is performed before sintering, and the pre-sintering temperature is 600°C.
[0063] refer to Figure 1 , Figure 1This is a green body image of Al2O3 / SiC composite ceramics obtained by tape casting in an organic solvent system. Sintering can be vacuum sintering, hot pressing sintering under argon protective atmosphere, or isostatic pressing sintering. Due to the difficulty in densifying composite materials, pressure-assisted technology is usually required, such as hot pressing (HP) or glass encapsulation hot isostatic pressing (HIP), preferably hot pressing sintering, with a sintering temperature of 1500℃~1850℃. The sintering pressure is 20~50Mpa, and the pressure is maintained for 1h-2h.
[0064] refer to Figure 2 and Figure 3 , Figure 2 The invention is to prepare the XRD spectrum of Al2O3 / SiC composite ceramics. Figure 3 This is a schematic diagram of the microstructure of the prepared Al2O3 / SiC composite ceramic. The pre-sintering-HIP consolidation method can be regarded as a promising way to manufacture fully dense Al2O3 / SiC ceramics with submicron microstructure and high SiC content. The purpose of the pre-sintering stage is to remove these organic binder components at a lower temperature, such as usually 500℃-600℃, to avoid pores and defects during high-temperature sintering. Pre-sintering can also partially sinter the green body to increase its mechanical strength, thereby reducing the risk of damage during subsequent handling and hot pressing sintering. The pre-sintered body has a certain strength, but its density is still lower than the theoretical density and the porosity is high. Secondary sintering, especially hot pressing sintering, is carried out at higher pressure and temperature, which can significantly increase the density of the material and reduce the porosity, thereby greatly improving its mechanical properties and heat resistance. High temperature and pressure are conducive to the growth and phase change of grains, making the microstructure of the material more perfect and further improving the performance. The experimental process found that at the same temperature, as the volume fraction of SiC in the composite material increases from 0 to 10wt%, the difficulty of densification will increase. The volume density of the ceramic decreases from 99.9% to 95% with the increase of the amount of SiC. At the same time, it can be predicted that SiC inclusions will have a significant hindering effect on grain growth, which will lead to the formation of a special microstructure. When the volume fraction of SiC is very high, the alumina matrix is interspersed with infiltrated SiC networks. According to the percolation theory, the pressure resistance of the composite ceramic decreases under high pressure. When the pressure is 25Mpa, as the temperature increases from 1500℃ to 1800℃, the ceramic grain size is 1-2μm, the density of the composite material increases from 3.68 to 3.89, the maximum bending strength can reach 900Mpa, the Vickers hardness reaches 30Gpa, and the compressive strength is 50kV / mm (15kV / 0.3mm).
[0065] The present invention prepares nano-alumina and silicon carbide by tape casting and sintering; (1) nano-powders are difficult to form by ordinary molding methods due to their small particle size and large specific surface area, and excessive organic matter content in the organic solvent system is not conducive to molding. By optimizing material selection and process treatment in the early stage, a slurry system for stable tape casting is created. Through tape casting, composite ceramics can be formed in batches, greatly improving production efficiency; (2) Based on theory and reality, through treatment, alumina / silicon carbide is easier to disperse in the organic system, and electrostatic chuck dielectric layer ceramics with excellent mechanical and electrical properties are prepared; (3) The product obtained by tape casting has good uniformity and adjustable thickness, which is convenient for macroscopically regulating the microstructure of the electrostatic chuck; (4) In view of the difficulty in densification of multi-phase ceramics, a pre-sintering-HIP consolidation method is adopted to further improve the volume density of nano-composite ceramics and solve the technical problem of sintering Al2O3 / SiC ceramics.
[0066] The embodiments of the present invention are described in detail above with reference to the accompanying drawings, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the scope of protection of the present invention.
Claims
1. A method for preparing high-performance alumina composite ceramics, characterized in that: The preparation method comprises: Powder pretreatment: Process the nano silicon carbide powder and then pre-disperse it in a horizontal ball mill, add a dispersant to destroy the hard agglomerates and soft agglomerates in the powder to make it dispersed evenly, and disperse the nano alumina powder; The treated powder needs to be tested for the content of other substances. Among other substances, the content of surface metal impurities is less than 100ppm; The content of silicon carbide in the powder pretreatment is 0-10wt%, and the content of aluminum oxide is 90-100wt%; Sol: First add 0-60 parts of toluene, 0-20 parts of isopropanol and 1-5 parts of plasticizer into a pneumatic sol machine, slowly and evenly stir for 5-20 minutes, then slowly add 30-50 parts of PVB resin powder in small amounts several times, stir at high speed for 2-4 hours to ensure that the PVB resin powder is evenly and fully dissolved to form PVB colloid; Dispersion: First weigh a certain amount of balls, toluene and n-butanol mixed solvent into a stirred mill, with the ratio of toluene to n-butanol being 3:1 to 1:1, then add the pretreated nano-silicon carbide and nano-alumina powders and additives in sequence, turn on the stirring switch and stir for 1 to 4 hours; Mixing: transfer the alumina and silicon carbide slurry in the stirred mill to the drum ball mill, add a certain amount of PVB colloid according to the formula, and run at a certain stirring rate for 24 hours; Vacuum degassing: The slurry in the drum ball mill is sent into the degassing tank with N2 gas pressure, the viscosity of the slurry and the corresponding ambient temperature are measured, the water bath temperature is set according to the slurry viscosity and temperature, and the appropriate degassing vacuum degree and time are set. After the slurry is effectively degassed, it is aged for a period of time for use; Molding and sintering: Set the scraper blade height to 0.3-0.6mm, the casting speed to 0-300mm / min, set the temperature and inlet and outlet air flux according to the environment, and set the temperature of the drying zone of the casting machine to 0-100℃. According to the type of silicon carbide powder, the slurry is cast to obtain gray-black, gray-white or green cast green billets through casting, and then cut, punch, print, laminate and isostatically press to obtain block green billets for secondary molding, and finally debinding and sintering.
2. The method for preparing a high-performance alumina composite ceramic according to claim 1, characterized in that: The nano silicon carbide powder is α-SiC or β-SiC, the particle size of the α-SiC or β-SiC is 60nm-400nm, wherein the particle size D50 is 100-200nm, D10 is 30-50nm, D90 is 150-200nm, and D90 / D10 is 3-6.
3. The method for preparing a high-performance alumina composite ceramic according to claim 1, characterized in that: In the forming and sintering steps, the sintering is vacuum sintering or hot pressing sintering or isostatic pressing sintering under an argon protective atmosphere.
4. The method for preparing a high-performance alumina composite ceramic according to claim 2, characterized in that: The sintering is hot pressing sintering under argon protective atmosphere, the sintering temperature is 1500℃~1850℃, the sintering pressure is 20~50Mpa, the pressure is maintained for 1~2h, and then cooled to room temperature. Pre-sintering is performed before sintering, and the pre-sintering temperature is 550℃~600℃.
5. The method for preparing a high-performance alumina composite ceramic according to claim 1, characterized in that: The plasticizer is dibutyl phthalate, di-n-octyl phthalate or butyl benzyl phthalate, and the content of the plasticizer is 0-8wt%.
6. The method for preparing a high-performance alumina composite ceramic according to claim 1, characterized in that: The dispersant is PEG or fish oil or lecithin or oleic acid or oleic acid amide, and the content of the dispersant is 0-5wt%.
7. The method for preparing a high performance alumina composite ceramic according to claim 1, characterized in that: The alumina powder is nanometer high-purity alumina powder, gamma or alpha phase spherical particles, with a purity greater than or equal to 99.99%, a particle size D50=100-400nm, and BET=5-30m2 / g.
8. The method for preparing a high performance alumina composite ceramic according to claim 1, characterized in that: The α-SiC or β-SiC is nanometer high-purity silicon carbide, which is spherical particles of α phase or β phase or both, with a purity greater than or equal to 99.99%. The appearance color of silicon carbide is black, green or grayish white, the particle size D50 is 50-300nm, BET is 6-38m2 / g, and the volume fraction of silicon carbide accounts for 0-20% of the total.
Citation Information
Patent Citations
Bionic layered alumina morphology composite ceramic material based on nano-texture toughening, and preparation method of composite ceramic material
CN109534792A
High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof
CN114538900A
Alumina ceramic as well as preparation method and application thereof
CN115340367A
High-purity high-strength aluminum oxide ceramic substrate and preparation method thereof
CN115849885A
SiC-Al2O3 composite sintered bodies and method of producing the same