High-performance sintered ferrite magnet and preparation method thereof

Through the new ball milling process and gradient heating sintering process, the problem of difficult dispersion of rare earth elements in ferrite materials is solved, the uniformity and performance of magnets are improved, the production cost is reduced, and the preparation of high-performance sintered ferrite magnets is realized. .

CN118930243AInactive Publication Date: 2024-11-12ANHUI ONE MAGNET ELECTRONIC CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411073526.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

Smart Images

  • Figure CN118930243A_ABST
    Figure CN118930243A_ABST
Patent Text Reader

Abstract

The invention discloses a high-performance sintered ferrite magnet and a preparation method thereof, and belongs to the technical field of rare earth magnetic materials. The method comprises the following steps: carrying out primary ball milling on preparation raw materials and water, drying, pre-sintering, crushing and sieving to obtain pre-sintered material particles, mixing the pre-sintered material particles with calcium carbonate, silicon dioxide, boric acid, kaolin and a dispersing agent, carrying out secondary ball milling, adding a magnetic field for orientation, carrying out wet compression molding to obtain a green body, and finally carrying out sintering molding to obtain the high-performance sintered ferrite magnet. Bearing steel balls are adopted for ball milling, and the magnetic performance of a product obtained through ball milling is obviously better than that of a product obtained through alloy steel ball milling; the preparation method comprises the following steps: selecting bearing steel balls of 6 mm and 4.8 mm according to a ratio of 4: 6, selecting the rotating speed of a ball mill to be 22r / min, and carrying out ball milling for 10 hours, so that the obtained slurry has the best magnetic performance and good particle size distribution, and can be used for preparing a high-performance sintered ferrite magnet.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rare earth permanent magnet materials, and in particular relates to a high-performance sintered ferrite magnet and a preparation method thereof. Background Art

[0002] Ferrite permanent magnet materials are cheap, have the advantages of high temperature resistance and corrosion resistance, and have a wide range of applications. For example, electronic products, automobiles, home appliances and other industries have a wide range of demands for them. At present, the country advocates energy conservation, environmental protection and green development, and permanent magnet materials are increasingly widely used in emerging fields such as new energy, electric vehicles, smart cities, and smart earth. The mainstream production process of high-performance ferrite materials is based on iron red pre-sintered materials. In the process of secondary mixing and fine grinding, a small amount of rare earth elements are added, magnetized, pressed and sintered, and finally the finished ferrite material is obtained after grinding. However, there are some defects in the current mainstream production process of mid-to-high-end ferrite materials: in the process of secondary mixing and grinding, the small amount of rare earth elements added is difficult to disperse effectively. Excessive mixing and grinding time will increase energy consumption and may cause over-grinding, thereby affecting the particle size distribution of the slurry, and ultimately resulting in reduced magnetic properties of the finished ferrite product. The external dependence of iron red is high, so the production cost of iron red pre-sintered materials is relatively high. The particle size distribution of the secondary mixing and grinding slurry has an important influence on the secondary generation and perfection of ferrite crystals. The traditional method of controlling the slurry particle size distribution by simply controlling the secondary mixing time has the problem of a wide distribution of slurry particle sizes.

[0003] Highly stable permanent ferrite materials cannot be prepared using traditional production methods, so it is necessary to develop a high-performance sintered ferrite magnet material and a preparation method thereof to reduce production costs and improve stability. Summary of the invention

[0004] The object of the present invention is to provide a high-performance sintered ferrite magnet and a preparation method thereof, so as to solve the problem that the prior art is high in cost and difficult to prepare high-performance sintered ferrite magnets.

[0005] A high performance sintered ferrite magnet and a preparation method thereof, comprising the following steps:

[0006] S1. Using a new ball milling process, the raw materials and water are weighed and mixed, and then ball milled to obtain a primary ball milling slurry;

[0007] S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles;

[0008] S3. The pre-sintered material particles are mixed with calcium carbonate, silica, boric acid, kaolin and a dispersant, finely ground and mixed to obtain a secondary ball-milled slurry;

[0009] S4. Orienting the secondary ball-milled slurry with a magnetic field and wet pressing to obtain a green embryo;

[0010] S5. Dry the green body by using an optimized sintering process, and then gradually increase the temperature to 1080-1120° C. to obtain the permanent ferrite.

[0011] Furthermore, the raw materials prepared in S1 are ferric oxide and rare earth oxide, with the mass fraction accounting for 92-96%:4-8%.

[0012] Furthermore, the rare earth oxide in S1 is one or more of the oxides of La, Pr, Dy, Tb and Ce.

[0013] Furthermore, the ball mill steel in S1 is bearing steel balls, the diameters of the bearing steel balls are 6 mm and 4.8 mm respectively, and the quantity ratio is 4:6.

[0014] Furthermore, the volume ratio of the ball milling medium, preparation principle and water in S1 is 90-92%: 4-5%: 4-5%, the ball mill speed is 18-22r / min, and the ball milling time is 9-11h.

[0015] Furthermore, the pre-burning temperature in S2 is 1200-1280° C., the heating time is 6-6.5 h, and the heat preservation time is 0.5-1 h.

[0016] Furthermore, the mesh size of the crushed and sieved sieve in S2 is 100 meshes.

[0017] Furthermore, the dispersants in S3 are calcium gluconate and sorbitol, and the mass fraction of calcium gluconate is 0.025-0.05%.

[0018] Furthermore, the volume ratio of the ball milling media in S3: pre-sintered material particles, calcium carbonate, silicon dioxide, boric acid, kaolin, water and dispersant is 68-70%: 18-20%: 1-2%: 1-2%: 1-2%: 1-2%: 1-2%: 1-2%, the ball mill speed is 18-22r / min, and the ball milling time is 9-11h.

[0019] Furthermore, in S5, the gradient heating starts from room temperature, is heated to 500°C at 15°C / min, is kept warm for 2 hours, and then starts from 500°C, is heated to 1100°C at 15°C / min, and is kept warm for 3 hours.

[0020] A high-performance sintered ferrite magnet is prepared by the above preparation method.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] 1. The present invention adopts an optimized steel ball ratio scheme, selects 6mm and 4.8mm bearing steel balls in a ratio of 4:6, and selects the ball mill speed to be 18-22r / min, and the ball milling is performed for 10 hours, which can improve the ball milling efficiency and reduce energy consumption, while ensuring the uniformity and fineness of the magnet components, providing a good foundation for the subsequent sintering process. The obtained slurry has the best magnetic properties and the slurry particle size distribution is good.

[0023] 2. The present invention adopts a gradient temperature rise sintering method to achieve high density and excellent performance of the magnet. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a flow chart of a high performance sintered ferrite magnet and a preparation method thereof according to an embodiment of the present application. DETAILED DESCRIPTION

[0025] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Embodiment 1:

[0027] See also Figure 1 , a high performance sintered ferrite magnet and a preparation method thereof, comprising the following steps:

[0028] S1. Using a new ball milling process, the raw materials and water are weighed and mixed, and then ball milled, wherein the volume ratio of the ball milling medium, the raw materials and water is 90%:5%:5%, the ball mill speed is 18r / min, and the ball milling time is 5h, to obtain a primary ball milled slurry;

[0029] S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles;

[0030] S3. The pre-sintered particles are mixed with calcium carbonate, silicon dioxide, boric acid, kaolin and a dispersant in a weight ratio of 70%: 18%: 2%: 2%: 2%: 2%: 2%: 2% respectively, and finely ground and mixed to obtain a secondary ball milling slurry; the ball mill speed is 19 r / min, and the ball milling time is 10 h;

[0031] S4. Orienting the secondary ball-milled slurry with a magnetic field and wet pressing to obtain a green embryo;

[0032] S5. Dry the green body by using an optimized sintering process, and then gradually increase the temperature to 1100° C. to obtain the permanent ferrite.

[0033] Embodiment 2:

[0034] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the volume ratio of the ball milling medium, the preparation raw material and water in S1 is 90%:5%:5%, the ball mill speed is 20r / min, the ball milling time is 10h, and the other components and parameters remain unchanged.

[0035] Embodiment 3:

[0036] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the volume ratios of the ball milling medium, the preparation raw materials and water in S1 are 92%:4%:4%, the ball mill speed is 18 r / min, the ball milling time is 10 h, and the other components and parameters remain unchanged.

[0037] Embodiment 4:

[0038] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the volume ratios of the ball milling medium, the preparation raw materials and water in S1 are 92%:4%:4%, the ball mill speed is 20r / min, the ball milling time is 10h, and the other components and parameters remain unchanged.

[0039] Embodiment 4:

[0040] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the volume ratios of the ball milling medium, the preparation raw materials and water in S1 are 92%:4%:4%, the ball mill speed is 22r / min, the ball milling time is 10h, and the other components and parameters remain unchanged.

[0041] Embodiment 5:

[0042] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that of Example 1, except that the volume ratio of the ball milling media in S3: pre-sintered material particles, calcium carbonate, silicon dioxide, boric acid, kaolin, water and dispersant is 70%: 20%: 2%: 2%: 2%: 2%: 1%: 1%, the ball mill speed is 20 r / min, the ball milling time is 10 h, and the other components and parameters remain unchanged.

[0043] Embodiment 6:

[0044] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that of Example 1, except that the volume ratio of the ball milling media in S3: pre-sintered material particles, calcium carbonate, silicon dioxide, boric acid, kaolin, water and dispersant is 70%: 20%: 2%: 2%: 2%: 2%: 1%: 1%, the ball mill speed is 22 r / min, the ball milling time is 10 h, and the other components and parameters remain unchanged.

[0045] Embodiment 7:

[0046] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the volume ratio of ball milling medium, preparation raw materials and water in S1 is 92%:4%:4%, the ball mill speed is 22r / min, and the ball milling time is 10h; the volume ratio of ball milling medium: pre-sintered material particles, calcium carbonate, silicon dioxide, boric acid, kaolin, water and dispersant in S3 is 70%:20%:2%:2%:2%:2%:1%:1%, the ball mill speed is 22r / min, and the ball milling time is 10h, and the other components and parameters remain unchanged.

[0047] Comparative Example 1:

[0048] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the steel used for ball milling in S1 is an alloy steel ball, the diameter of the alloy steel ball is 5 mm, and the other components and parameters remain unchanged.

[0049] Comparative Example 2:

[0050] A high-performance sintered ferrite magnet and a preparation method thereof. The preparation method is the same as that in Example 1, except that the sintering in S5 adopts a traditional heating method, heating from 25°C to 1100°C at a heating rate of 15°C / min, and keeping the temperature for 2h, while the other components and parameters remain unchanged.

[0051] The magnet properties of the above different embodiments and comparative examples were tested at 25° C. The test results are shown in Table 1.

[0052] Table 1

[0053]

[0054] It can be seen from Table 1 that by adopting an optimized steel ball ratio scheme, selecting 6mm and 4.8mm bearing steel balls in a ratio of 4:6, the ball milling efficiency can be improved, energy consumption can be reduced, and the uniformity and fineness of the magnet components can be ensured, while the comprehensive magnetic properties can be maximized. It can be seen from Examples 1-7 and Comparative Example 1 that with the continuous increase in the rotation speed of the primary and secondary ball mills, the comprehensive performance of the magnet is also continuously improved. It can be seen from Comparative Example 2 that the high density and excellent performance of the magnet can be achieved by using a gradient temperature rise sintering method instead of a traditional temperature rise sintering method.

[0055] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0056] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A high performance sintered ferrite magnet and a preparation method thereof, characterized in that: The following steps are involved: S1. Using a new ball milling process, the raw materials and water are weighed and mixed, and then ball milled to obtain a primary ball milling slurry; S2. The primary ball-milled slurry is dried, pre-calcined, crushed and sieved to obtain pre-calcined particles; S3. The pre-sintered material particles are mixed with calcium carbonate, silica, boric acid, kaolin, water and a dispersant, and finely ground and mixed to obtain a secondary ball-milled slurry; S4. Orienting the secondary ball-milled slurry by adding a magnetic field, and wet pressing to obtain a green embryo; S5. Dry the green body by using an optimized sintering process, and then gradually increase the temperature to 1080-1120° C. to obtain the permanent ferrite.

2. A high performance sintered ferrite magnet and a preparation method thereof according to claim 1, characterized in that: The raw materials prepared in S1 are ferric oxide and rare earth oxide, with the mass fraction accounting for 92-96%:4-8%.

3. A high performance sintered ferrite magnet and a method for preparing the same according to claim 2, characterized in that: The rare earth oxide in S2 is one or more of the oxides of La, Pr, Dy, Tb and Ce.

4. A high performance sintered ferrite magnet and a method for preparing the same according to claim 1, characterized in that: The ball mill steel in S1 is bearing steel balls, the diameters of the bearing steel balls are 6 mm and 4.8 mm respectively, and the quantity ratio is 4:

6.

5. A high performance sintered ferrite magnet and a method for preparing the same according to claim 1, characterized in that: The volume proportions of the ball milling medium, the preparation raw materials and the water in S1 are 90-92%: 4-5%: 4-5%, the ball mill speed is 18-22r / min, and the ball milling time is 9-11h.

6. A high performance sintered ferrite magnet and a method for preparing the same according to claim 1, characterized in that: The pre-burning temperature in S2 is 1200-1280° C., the heating time is 6-6.5 hours, and the heat preservation time is 0.5-1 hour.

7. A high performance sintered ferrite magnet and a method for preparing the same according to claim 1, characterized in that: The mesh number of the crushed and sieved sieve in S2 is 100 meshes.

8. A high performance sintered ferrite magnet and a method for preparing the same according to claim 1, characterized in that: The dispersants in S3 are calcium gluconate and sorbitol, and their mass fractions are both 0.025-0.05%; the ball milling media in S3: pre-sintered material particles, calcium carbonate, silicon dioxide, boric acid, kaolin, water and dispersant have a volume ratio of 68-70%: 18-20%: 1-2%: 1-2%: 1-2%: 1-2%: 1-2%: 1-2%, the ball mill speed is 18-22r / min, and the ball milling time is 9-11h.

9. A highly stable permanent magnetic ferrite material and a preparation method thereof according to claim 1, characterized in that: In the S5, the temperature is gradually increased from room temperature to 500°C at a rate of 15°C / min, and then kept at this temperature for 2 hours. Then, the temperature is gradually increased from 500°C to 1100°C at a rate of 15°C / min, and then kept at this temperature for 3 hours.

10. A high performance sintered ferrite magnet, characterized in that: Prepared by the production process described in any one of claims 1 to 10.

Citation Information

Patent Citations

  • Preparation method of high-performance permanent magnetic ferrite

    CN112209707A

  • Preparation method of permanent magnetic ferrite and permanent magnetic ferrite

    CN112876231A

  • Magnetic powder

    WO2016165305A1