Thin film thermocouple preparation method based on indium tin oxide composite nanoparticles

By using indium tin oxide composite nanoparticles in ITO-In2O3 film thermocouples, the problem of low Seebeck coefficient and easy cracking in inkjet printing film thermocouples is solved, and higher Seebeck coefficient and fewer surface cracks are achieved. Improves the density and high temperature stability of the film.

CN118930248APending Publication Date: 2024-11-12BEIHANG UNIV
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411012273.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing inkjet printing produced ITO-In2O3 film thermocouple has low Seebeck coefficient and is prone to cracks, resulting in insufficient temperature measurement sensitivity and poor stability.

Method used

Indium tin oxide composite nanoparticles are used to mix ITO nanoparticles with In2O3 nanoparticles and disperse them into organic solvents to form ITO-In2O3 composite nanoparticles ink, and printed on the substrate surface using inkjet printing and high-temperature thermal sintering to make nanometers The particles are connected to each other to form a conductive network.

Benefits of technology

The Seebeck coefficient of the film thermocouple is improved, the surface cracks are reduced, the density and high temperature stability of the film are enhanced, and the temperature measurement sensitivity is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930248A_ABST
    Figure CN118930248A_ABST
Patent Text Reader

Abstract

A thin film thermocouple preparation method based on indium tin oxide composite nanoparticles belongs to the field of thin film thermocouple manufacturing, and comprises the following steps: mixing ITO nanoparticles and In2O3 nanoparticles, dispersing the mixture into an organic solvent, and performing ultrasonic treatment and filtration to prepare ITO-In2O3 composite nanoparticle ink; the preparation method comprises the following steps: dispersing In2O3 nanoparticles into an organic solvent, and performing ultrasonic treatment and filtration to prepare In2O3 nanoparticle ink; the method comprises the following steps: printing an ITO (Indium Tin Oxide)-In < 2 > O < 3 > composite nanoparticles-In < 2 > O < 3 > thin film thermocouple on a substrate by using ITO-In < 2 > O < 3 > composite nanoparticle ink and In < 2 > O < 3 > nanoparticle ink And the nano-particles are mutually connected to form a conductive network through high-temperature thermal sintering. The thin film thermocouple prepared by the invention has a relatively high Seebeck coefficient and fewer surface cracks, and the high-temperature stability of the thin film is ensured. The porosity of the film can be effectively reduced, and the density of the film is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thin film thermocouple manufacturing, and in particular relates to a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles. Background Art

[0002] Thin film thermocouples are small in size (about 1 μm thick) and have little interference with the measured temperature field, so they are widely used in fields such as turbine blade temperature measurement. Using inkjet printing to make thin film thermocouples is an emerging and flexible method for processing thin film thermocouples.

[0003] Thermoelectric materials are usually prepared as nanoparticles and dispersed in a solvent to form ink, which is then directly printed on the surface of a substrate to form a thin film thermocouple. The Seebeck coefficient and the stability of high temperature measurements are the two most important criteria for measuring the performance of thin film thermocouples. 2 O 3 Semiconductor metal oxide materials such as quartz and tantalum have excellent high temperature resistance and oxidation resistance, and are therefore the most commonly used thermoelectric materials.

[0004] Currently, ITO-In made by inkjet printing 2 O 3 Thin film thermocouple (one branch uses ITO and the other branch uses In 2 O 3 ) There are two main technical problems. On the one hand, the Seebeck coefficient of thin-film thermocouples is lower than that of thermocouples of the same material made by PVD process (the former is usually less than 100μV / K, while the latter can be up to more than 200μV / K). On the other hand, due to the characteristics of ITO material itself, ITO film made by inkjet printing is extremely prone to cracks, which will cause the thin-film thermocouple to fail.

[0005] In summary, there is an urgent need to develop a method that can both increase the Seebeck coefficient of the thin film thermocouple to enhance its temperature measurement sensitivity and eliminate cracks in the thin film thermocouple. Summary of the invention

[0006] In order to solve the existing ITO-In 2 O 3 The thin film thermocouple has a lower Seebeck coefficient than the thermocouple of the same material made by PVD process and the ITO film made by inkjet printing is prone to cracks, resulting in failure of the thin film thermocouple. The present invention provides a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles.

[0007] The technical solution adopted by the present invention to solve the technical problem is as follows:

[0008] The present invention provides a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles, which specifically comprises the following steps:

[0009] ITO nanoparticles and In 2 O 3 The nanoparticles are mixed and dispersed in an organic solvent, and then ultrasonicated and filtered to prepare ITO-In 2 O 3 Composite nanoparticle ink; In 2 O 3 The nanoparticles are dispersed in an organic solvent, and then ultrasonicated and filtered to prepare In 2 O 3 Nanoparticle ink; using ITO-In 2 O 3 Composite nanoparticle ink and In 2 O 3 Nanoparticle ink is printed on the substrate surface by inkjet printing. 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple; after high temperature thermal sintering, the nanoparticles are connected to each other to form a conductive network.

[0010] The organic solvent is preferably a mixed solution of ethylene glycol and isopropanol, and the mass ratio of ethylene glycol to isopropanol is preferably 0.8-1.

[0011] Wherein, the ITO nanoparticles and In 2 O 3 The mass ratio of the nanoparticles is 4:1 to 19:1.

[0012] Wherein, the ITO-In 2 O 3 The mass fraction of the composite nanoparticle ink is preferably 10% to 20%.

[0013] The ultrasonic parameters are preferably: power 120W to 200W, time 2 hours to 4 hours.

[0014] Wherein, the filtration is preferably performed using a 0.45 μm PTFE filter membrane.

[0015] Among them, the In 2 O 3 The mass fraction of the nanoparticle ink is preferably 10% to 20%.

[0016] Wherein, the substrate is preferably Al 2 O 3 Ceramic substrate or Si ceramic substrate.

[0017] Wherein, the temperature of the substrate is preferably 140°C to 160°C.

[0018] The high temperature sintering is preferably carried out at a temperature of 1000° C. to 1200° C. and for a time of 25 min to 35 min.

[0019] The beneficial effects of the present invention are:

[0020] (1) ITO-In prepared by the present invention 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouples have a higher Seebeck coefficient, which is at least 13.4% higher than that of ordinary thermocouples.

[0021] (2) ITO-In prepared by the present invention 2 O 3 Composite Nanoparticles-In 2 O 3 Compared with ITO thin film, thin film thermocouple has fewer surface cracks, thus ensuring the high temperature stability of the film.

[0022] (3) The present invention can effectively reduce the porosity of the film and improve the density of the film.

[0023] (4) The preparation process of the present invention is simple and the film effect is obvious. It is a very simple and optimized preparation method of inkjet printed thin film thermocouples. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The microscopic morphology of the nanoparticle film. In the figure, (a) SEM image and binary image of ITO nanoparticle film; (b) In 2 O 3 SEM image and binary image of nanoparticle film; (c) ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 SEM images and binarization images of the film.

[0025] Figure 2 The comparison chart of film mobility. In the figure, (a) ITO nanoparticle film; (b) In 2 O 3 Nanoparticle film; (c) ITO-In 2 O 3 Composite nanoparticle films.

[0026] Figure 3 This is a comparison chart of the thermoelectric characteristics of thermocouples.

[0027] Figure 4 The crack images on the film surface. In the figure, (a) ITO nanoparticle film; (b) ITO-In 2 O 3 Composite nanoparticle films. DETAILED DESCRIPTION

[0028] The technical solutions of the present invention will be described clearly and completely below in conjunction with specific embodiments of the present invention.

[0029] The present invention provides a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles, which mainly comprises the following steps:

[0030] (1) Preparation of ITO-In 2 O 3 Composite nanoparticle ink: ITO nanoparticles and In 2 O 3 The nanoparticles are mixed and dispersed in an organic solvent, and then ultrasonicated and filtered to prepare ITO-In 2 O 3 Composite nanoparticle inks for inkjet printing.

[0031] The specific operation process is as follows:

[0032] ITO nanoparticles (average particle size 30nm) and In 2 O 3 Nanoparticles (average particle size 100 nm) are mixed and dispersed in a mixed solution composed of ethylene glycol and isopropanol, wherein the mass ratio of ethylene glycol to isopropanol is preferably 0.8 to 1, and the ITO nanoparticles and In 2 O 3 The mass ratio of nanoparticles is 4:1 to 19:1, and the obtained ITO-In 2 O 3 The mass fraction of the composite nanoparticle ink is 10% to 20%; then the obtained ITO-In 2 O 3 The composite nanoparticle ink is ultrasonically treated, the ultrasonic power is set to 120W to 200W, and the ultrasonic dispersion is performed for 2 hours to 4 hours; finally, a 0.45 μm PTFE filter membrane is used.

[0033] (2) Preparation of In 2 O 3 Nanoparticle ink: ITO nanoparticles are dispersed in an organic solvent, and then ultrasonically and filtered to prepare In 2 O 3 Nanoparticle inks for inkjet printing.

[0034] The specific operation process is as follows:

[0035] In 2 O 3 The nanoparticles are dispersed in a mixed solution of ethylene glycol and isopropanol, wherein the mass ratio of ethylene glycol to isopropanol is preferably 0.8 to 1. 2 O 3 The mass fraction of the nanoparticle ink is 10% to 20%; then the obtained In 2 O 3 The nanoparticle ink is ultrasonically treated, the ultrasonic power is set to 120W to 200W, and the ultrasonic dispersion is performed for 2 hours to 4 hours; finally, a 0.45 μm PTFE filter membrane is used.

[0036] (3) Inkjet printing: ITO-In is directly deposited on the substrate surface with high uniformity through inkjet printing technology. 2 O 3 Composite nanoparticle films and In 2 O 3 Nanoparticle film, preparation of ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple.

[0037] The specific operation process is as follows:

[0038] Before inkjet printing, Al 2 O 3 The ceramic substrate was ultrasonically cleaned, specifically using isopropyl alcohol, ethanol and ultrapure water for 3 minutes each, and then dried with a hot air gun. ITO-In was prepared under the waveform conditions of positive voltage 70V-80V, negative voltage 70V-100V, reference voltage 5V, positive voltage rise time 12ms, positive voltage duration 30ms-40ms, positive voltage drop time 20ms-30ms, negative voltage duration 30ms-40ms, and negative voltage rise time 5ms-8ms. 2 O 3 Stable droplets of composite nanoparticle ink and In 2 O 3 Stable droplets of nanoparticle ink. Al 2 O 3 The temperature of the ceramic substrate is 140° C. to 160° C. The printing parameters and printing pattern are set, wherein the printing parameters are preferably: the horizontal printing dot spacing is 0.04 mm to 0.05 mm, the vertical printing dot spacing is 0.04 mm to 0.05 mm, and the printing rate is 10 mm / s to 20 mm / s; the printing pattern is preferably a 150 mm×2 mm long strip film.

[0039] (4) High temperature thermal sintering: The high temperature thermal sintering process is used to connect the nanoparticles to form a conductive network.

[0040] The specific operation process is as follows:

[0041] The obtained ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple with Al 2 O 3 The ceramic substrate is placed in a temperature-controlled tubular sintering furnace, and the high-temperature sintering temperature is set to 1000℃~1200℃, the time is 25min~35min, and the heating program of the tubular sintering furnace is started to perform high-temperature sintering in an air atmosphere. After the heating program is completed, the tubular sintering furnace is cooled to room temperature, and the thin film thermocouple is taken out. At this point, the ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple preparation.

[0042] The present invention provides a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles. First, a certain proportion of In is added to the ITO nanoparticles. 2 O 3 Nanoparticles, making ITO-In 2 O 3 Composite nanoparticle ink, combined with In 2 O 3 Nanoparticle ink, making ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple. Experiments have shown that this new type of ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouples have lower porosity, higher Seebeck coefficient, and better film quality.

[0043] Among them, ITO nanoparticles (average particle size of 30nm) film, In 2 O 3 Nanoparticle (average particle size 100nm) film and ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 The microscopic morphology of the film Figure 1 As shown, according to the binary SEM image, ITO-In2 O 3 Composite Nanoparticles-In 2 O 3 The film has lower porosity, ITO nanoparticle film and In 2 O 3 Nanoparticle films all have high porosity, among which the porosity from low to high is: ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Film, In 2 O 3 Nanoparticle films and ITO nanoparticle films.

[0044] Among them, highly uniform ITO-In is directly deposited on the substrate surface by inkjet printing technology. 2 O 3 Composite nanoparticle films and In 2 O 3 Nanoparticle film makes ITO-In 2 O 3 Composite nanoparticle film and In 2 O 3 One end of the nanoparticle film overlaps each other to form ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouple; finally, high temperature thermal sintering process is used to connect the nanoparticles to form a conductive network, thereby generating thermoelectric properties. Figure 2 As shown, due to ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 The porosity of the film is reduced, and ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 The number of conductive paths in the thin film increases, which facilitates the migration of carriers and rapidly increases the mobility by an order of magnitude. 2 O 3 Composite Nanoparticles-In 2 O 3 The thermoelectric properties of thin film thermocouples are significantly higher than those of ordinary ITO-In 2 O 3 Thermocouple. Figure 3 "Pure ITO" means traditional ITO-In 2 O 3Thermoelectric output of thin film thermocouples, “In 2 O 3 :ITO=1:19(mass ratio)”,In 2 O 3 :ITO=1:9(mass ratio)”,In 2 O 3 :ITO=1:4 (mass ratio)" means ITO / In in the present invention 2 O 3 Mixed Nanoparticles-In 2 O 3 Thermoelectric output of thin film thermocouple. The ratio after the equal sign represents the ratio of ITO nanoparticles to In 2 O 3 The mixing ratio of nanoparticles. "Temperature" refers to the temperature of the sintering furnace, which is considered to be the temperature of the thermocouple hot node. Figure 3 As a result, the output of the new thermocouple involved in the present invention is significantly higher than that of the traditional thermocouple. 2 O 3 Composite Nanoparticles-In 2 O 3 Thin film thermocouples compared to ordinary ITO-In 2 O 3 Thermocouples have a higher Seebeck coefficient.

[0045] In addition, due to the incorporation of larger nanoparticles, ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 The thin film thermocouple has a stronger ability to resist the shrinkage of the liquid film, so ITO-In 2 O 3 Composite Nanoparticles-In 2 O 3 The surface cracks of thin film thermocouples are significantly reduced, such as Figure 4 shown.

[0046] ITO-In prepared by the present invention 2 O 3 Composite Nanoparticles-In 2 O 3 The thin film thermocouple has a higher Seebeck coefficient and fewer surface cracks, thus ensuring the high temperature stability of the film. At the same time, the invention effectively reduces the porosity of the film and improves the density of the film.

[0047] The present invention discloses a method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve it. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The product of the present invention has been described through a preferred embodiment, and relevant personnel can obviously modify or appropriately change and combine the product described herein without departing from the content, spirit and scope of the present invention to realize and apply the technology of the present invention.

Claims

1. A method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles, characterized in that: The following steps are involved: ITO nanoparticles and In2O3 nanoparticles are mixed and dispersed in an organic solvent, and then prepared into ITO-In2O3 composite nanoparticle ink after ultrasonication and filtration; In2O3 nanoparticles are dispersed in an organic solvent, and then prepared into In2O3 nanoparticle ink after ultrasonication and filtration; ITO-In2O3 composite nanoparticle ink and In2O3 nanoparticle ink are used to print ITO-In2O3 composite nanoparticle-In2O3 thin film thermocouples on the surface of a substrate by inkjet printing; and nanoparticles are connected to each other through high-temperature thermal sintering to form a conductive network.

2. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The organic solvent is a mixed solution of ethylene glycol and isopropanol, and the mass ratio of ethylene glycol to isopropanol is 0.8-1.

3. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The mass ratio of the ITO nanoparticles to the In2O3 nanoparticles is 4:1 to 19:

1.

4. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The mass fraction of the ITO-In2O3 composite nanoparticle ink is 10% to 20%.

5. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The ultrasonic parameters are: power 120W-200W, time 2 hours-4 hours; the filtration uses a 0.45 μm PTFE filter membrane.

6. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The mass fraction of the In2O3 nanoparticle ink is 10% to 20%.

7. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The substrate is an Al2O3 ceramic substrate or a Si ceramic substrate.

8. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The temperature of the substrate is 140°C to 160°C.

9. The method for preparing a thin film thermocouple based on indium tin oxide composite nanoparticles according to claim 1, characterized in that: The high temperature sintering temperature is 1000° C. to 1200° C., and the time is 25 min to 35 min.

Citation Information

Patent Citations

  • An indium tin oxide nanometer crystal composite solution, and a preparing method and applications thereof

    CN105776321A

  • Method for preparing indium tin oxide-indium oxide thin film thermocouple with crystal face preferred orientation

    CN113174568A

  • Preparation method of heavily doped ITO powder

    CN116621575A

  • Thin film thermocouple error compensation method based on recurrent neural network

    CN116698217A

  • Method for optimizing nano particle laser sintering characteristics based on ITO sacrificial layer

    CN117936392A