Preparation method and application of stretchable MXene thermoelectric fabric
By soaking the fabric in ethanol solution, modifying dopamine, cationic modification of chitosan and immersing of MXene dispersion, stretchable MXene thermoelectric fabric was prepared, which solved the poor breathability and comfort of the existing MXene thermoelectric composite film materials. Problem, efficient thermoelectric sensing and breathing monitoring are achieved.
Patent Information
- Application Number
- CN202411054367.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing MXene thermoelectric composite film materials have poor breathability, poor comfort and difficulty in sewing with fabrics, which limit their application scenarios.
The fabric is soaked with ethanol solution, followed by modification in dopamine solution and cationically modified in chitosan solution, and then MXene dispersion is obtained by etching and ultrasonic treatment, and finally the positively charged fabric is immersed in MXene dispersion. A stretchable MXene thermoelectric fabric was prepared in liquid.
The prepared MXene thermoelectric fabric has good electrical properties, elasticity and thermoelectric sensing stability. It can effectively convert the environment and human temperature difference into electrical energy, and can be sewn with a breathing mask to achieve monitoring and identification of respiratory status under different exercise states.
Smart Images

Figure CN119041196A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of thermoelectric fabric processing, and in particular relates to a preparation method and application of stretchable MXene thermoelectric fabric. Background Art
[0002] Wearable electronics have been widely used in various fields, including motion monitoring, health monitoring, human-computer interaction, and fitness and entertainment. However, traditional wearable electronics usually require external power or frequent charging, limiting their usability and portability. Therefore, it is becoming increasingly important to develop a self-powered sensing system that can harvest energy from the natural environment.
[0003] Recently, advances in energy harvesting technologies such as thermoelectric, triboelectric, and piezoelectric, as well as self-charging methods, have made significant progress in the field of wearable electronics. Among them, wearable thermoelectric devices that directly convert thermal energy into electrical energy have become a promising power source due to the ubiquity of temperature changes in the environment. Common thermoelectric materials such as carbon nanotubes, PEDOT:PSS (poly(3,4-ethylenedioxythiophene)-polystyrene sulfonate) and MXene (Ti3C2T x ) and other materials have good electrical conductivity and are easy to process, and are gradually becoming ideal choices for thermoelectric materials. Among them, two-dimensional transition metal carbide MXene has excellent physical and chemical properties, including excellent electrical conductivity (>5000S cm-1), excellent hydrophilicity, high interface thermal resistance and low in-plane thermal conductivity (~0.279Wm -1 K -1 ), making it ideal for use in wearable thermoelectric sensing devices.
[0004] At present, there are some flexible composite thermoelectric film materials based on MXene. For example, patent CN113224231A discloses a method for preparing a flexible MXene / PEDOT:PSS composite thermoelectric material; patent CN110713706A discloses a self-healing MXene / polyurethane thermoelectric composite material and its preparation method; patent CN116828951A discloses an n-type bismuth telluride flexible composite thermoelectric film, method and device based on a MXene substrate; however, these MXene-based thermoelectric composite films have problems such as poor air permeability, poor comfort and difficulty in sewing with fabrics, which limits their application scenarios. Summary of the invention
[0005] In order to solve the above problems, the present invention provides a method for preparing a stretchable MXene thermoelectric fabric, which specifically comprises the following steps:
[0006] (1) soaking the fabric in an ethanol solution to remove grease residue on the fiber surface, and drying to obtain the treated fabric;
[0007] (2) placing the fabric treated in step (1) into a dopamine solution for reaction, modifying the fabric by dopamine self-polymerization to obtain a polydopamine-modified fabric;
[0008] (3) immersing the polydopamine-modified fabric obtained in step (2) in a chitosan solution to perform cationic modification on the polydopamine-modified fabric to obtain a positively charged fabric;
[0009] (4) Lithium fluoride, hydrochloric acid and deionized water are stirred and mixed to etch Ti3AlC2, the precipitate is separated and collected, the precipitate is dispersed using an intercalation agent, ultrasonically treated, and centrifuged to collect the upper MXene dispersion;
[0010] (5) Immersing the positively charged fabric in step (3) in a MXene dispersion and drying to obtain a MXene thermoelectric fabric.
[0011] In one embodiment of the present invention, in step (1), the volume concentration of the ethanol solution is 30-70%, and the soaking time is 20-50 minutes, in order to remove the grease residue on the fiber surface.
[0012] In one embodiment of the present invention, in step (1), the fabric is one of nylon fabric, cotton fabric and ketone-ammonia fabric.
[0013] In one embodiment of the present invention, in step (2), the mass concentration of the dopamine solution is 0.5-1%, the pH is 8-8.5, the reaction temperature is 25-40° C., and the reaction time is 8-24 hours.
[0014] In one embodiment of the present invention, in step (3), the mass concentration of the chitosan solution is 0.1-1%, and the immersion time is 10-60 minutes.
[0015] In one embodiment of the present invention, in step (4), the addition ratio of Ti3AlC2, lithium fluoride, hydrochloric acid and deionized water is 1 (g): 1-1.5 (g): 12-25 (mL): 4.5 (mL); the stirring speed is 300-600 rpm; the etching temperature is 30-45°C, and the etching time is 18-28h.
[0016] In one embodiment of the present invention, in step (4), the concentration of hydrochloric acid is 12 mol / L.
[0017] In one embodiment of the present invention, in step (4), the intercalant for dispersing the precipitate is deionized water or dimethyl sulfoxide, the ultrasonic time is 1 to 2.5 hours, the centrifugal speed is 4000 to 6000 rpm, and the centrifugal time is 3 to 6 minutes.
[0018] In one embodiment of the present invention, in step (5), the concentration of the MXene dispersion is 5 to 25 mg / mL.
[0019] The present invention provides a MXene thermoelectric fabric prepared by the above method.
[0020] The present invention also provides a mask for human respiratory monitoring, the mask comprising a mask body and a strap, the mask body being connected to a MXene thermoelectric fabric sensor array, and the specific preparation method is as follows: copper wire, conductive silver paste and copper tape are used to connect the MXene thermoelectric fabric described in claim 8 in series to obtain a MXene thermoelectric fabric sensor array; and the MXene thermoelectric fabric sensor array is then connected to the mask body by a flat needle method to obtain a mask for human respiratory detection.
[0021] [Beneficial Effects]
[0022] (1) The single-layer MXene nanosheet prepared by the present invention has good electrical properties;
[0023] (2) The nylon fabric used in the present invention makes the MXene thermoelectric fabric have good elasticity, and a stretchable MXene thermoelectric fabric is prepared;
[0024] (3) The present invention uses polydopamine to modify the surface of the fabric fiber, making the fiber surface rough, which is beneficial to provide attachment sites for the MXene material and increase the MXene loading;
[0025] (4) The polydopamine-modified fabric is cationically modified by chitosan. The electrostatic attraction between chitosan and MXene can increase the loading amount of MXene material and the binding force between MXene and fiber. MXene is used to decorate the flexible fabric to construct a three-dimensional network structure of MXene thermoelectric fabric with a Seebeck coefficient of up to -12.3μV K -1 , and has good thermoelectric sensing stability, can use the temperature difference between the environment and the human body to effectively convert it into electrical energy, and can be applied to human breathing monitoring;
[0026] (5) The present invention can improve the output voltage of the device by connecting multiple MXene thermoelectric fabrics in series to form a thermoelectric sensor array;
[0027] (6) The MXene thermoelectric fabric prepared by the present invention can be sewn with a respiratory mask by utilizing the good flexibility, air permeability and comfort of the fabric substrate to monitor and identify the breathing state of the body under different motion states;
[0028] (7) The MXene thermoelectric fabric prepared by the present invention has a simple preparation process, low requirements on production equipment and low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a TEM image of MXene nanosheets in Example 1 of the present invention;
[0030] Figure 2 This is an AFM image of MXene nanosheets in Example 1 of the present invention;
[0031] Figure 3 This is a SEM image of the fiber surface of the nylon fabric of Example 1 of the present invention;
[0032] Figure 4 This is a SEM image of the surface of the MXene thermoelectric fabric fiber in Example 1 of the present invention;
[0033] Figure 5 This is a working principle diagram of MXene thermoelectric fabric in Example 1 of the present invention;
[0034] Figure 6 This is the output voltage diagram of the MXene thermoelectric fabric in Example 1 of the present invention;
[0035] Figure 7 This is a schematic diagram of the MXene thermoelectric fabric sensor array of the present invention;
[0036] Figure 8 This is a monitoring diagram of the MXene thermoelectric fabric of the present invention on the breathing state of the human body. DETAILED DESCRIPTION
[0037] Test method for fabric air permeability: The air permeability of fabric is tested using the YG461E air permeability instrument produced by Ningbo Textile Instrument Factory. The test standard is based on GB / T5453-1997 "Determination of fabric air permeability", using the constant pressure difference flow measurement method.
[0038] Test method for loading capacity: Before the test, a high-precision balance is used to record the initial weight of the sample and the weight after loading the MXene material, so as to obtain the loading capacity of the MXene conductive material.
[0039] Conductivity testing method: Use four probes to directly measure the MXene thermoelectric fabric to obtain the resistivity of the MXene thermoelectric fabric. The conductivity (S / m) of the MXene thermoelectric fabric can be calculated according to the formula "conductivity = 1 / resistivity".
[0040] Test method of Seebeck coefficient: Use voltage test instrument to record voltage difference between two ends of MXene thermoelectric fabric. Adjust the temperature of hot end of MXene thermoelectric fabric by controlling the temperature of constant temperature heating platform. Use handheld temperature gun and thermocouple to record the temperature of two ends of MXene thermoelectric fabric. Seebeck coefficient can be calculated by calculating temperature difference and open circuit voltage between two ends of MXene thermoelectric fabric.
[0041] Example 1
[0042] (1) placing a 1×20 cm nylon fabric in an ethanol solution with a volume concentration of 50% for 30 minutes, taking it out and placing it in a 60° C. vacuum drying oven for 20 minutes to obtain a treated nylon fabric;
[0043] (2) placing the nylon fabric treated in step (1) into a 0.8% dopamine solution, adjusting the solution pH to 8.5, reacting at a temperature of 35° C., shaking on a water bath shaker for 24 hours, taking it out and rinsing it with deionized water to remove residues, and drying it naturally at room temperature to obtain a polydopamine-modified nylon fabric;
[0044] (3) immersing the nylon fabric obtained in step (2) in a chitosan solution having a mass concentration of 0.5% for 30 minutes to perform cationic modification on the nylon fabric to obtain a nylon fabric with a positive charge;
[0045] (4) First, 2g LiF, 31mL HCl (12mol / L) and 9mL deionized water were added to a polytetrafluoroethylene beaker, and the whole was placed in a water bath thermostat with a water bath temperature of 35°C, a magnetic stirring speed of 400rpm, and a reaction time of 30min. Then, 2g Ti3AlC2 powder was slowly added to the above mixed solution, and the reaction lasted for 24h at 35°C. The obtained Ti3C2T x The product was washed with deionized water, each time at a centrifugal speed of 5000 rpm for 5 minutes, until the pH of the solution was close to neutral; then, deionized water was used as an intercalation agent, and the mixed solution was placed in an ultrasonic cleaning machine with a power of 500 W, and the ultrasonic cleaning was continued for 1 hour. Finally, the MXene dispersion was obtained by centrifugation at a speed of 5000 rpm for 5 minutes.
[0046] (5) The nylon fabric obtained in step (3) was placed in a 15 mg / mL MXene dispersion for 30 min, and then placed in a 50°C vacuum drying oven for 25 min to prepare a MXene thermoelectric fabric.
[0047] The conductivity of the MXene thermoelectric fabric prepared in Example 1 is 291.2 S / m, and the Seebeck coefficient is -12.3 μV K -1 , showing rapid thermoelectric response and excellent thermoelectric stability; under a pressure of 250Pa, the air permeability of the MXene thermoelectric fabric prepared in Example 1 is 130mm / s.
[0048] from Figure 1 It can be seen that MXene is in a flaky and transparent state; Figure 2This is the AFM of MXene nanosheets. From the thickness curve in the figure, it can be concluded that the thickness of the MXene nanosheet is about 1.6nm, indicating that a single layer of MXene nanosheets has been successfully prepared. Figure 3 This is a surface image of nylon fiber. It can be observed that the surface of the fiber is smooth. Figure 4 This is the morphology of MXene nanosheets wrapped on the surface of polydopamine-modified fibers. From the figure, it can be clearly observed that the MXene nanosheets are stacked on the surface of the fibers in a sheet state. Figure 5 The thermoelectric principle diagram of MXene thermoelectric fabric, the two ends of MXene thermoelectric fabric are in contact with the cold (unheated) source and the hot (heated) source respectively. The temperature difference between the two ends causes electrons to move from the hot end to the cold end, thereby generating a voltage difference. Figure 6 The voltage curve generated by the different temperature differences at both ends of the MXene thermoelectric fabric. It can be observed that the greater the temperature difference, the higher the output voltage.
[0049] Figure 7 This is the schematic diagram of the thermoelectric sensor array. By connecting MXene thermoelectric fabrics in series, the output voltage can be increased. The assembled MXene thermoelectric sensor array can not only increase the output voltage, but also accurately reflect the changes in the body's breathing signals.
[0050] A mask for human breathing detection includes a mask body and a strap, and a MXene thermoelectric fabric sensor array is connected to the mask body. The specific preparation method is as follows: four MXene thermoelectric fabrics prepared in Example 1 are connected in series using copper wire, conductive silver paste and copper tape to construct a MXene thermoelectric sensor array, and then the MXene thermoelectric fabric sensor array is connected to the mask body using a flat needle method, and the mask is put on to simulate the body's breathing information under different states. The voltage generated by the thermoelectric fabric can be tested by an electrochemical workstation and displayed on a computer to achieve the purpose of monitoring and identification. Figure 8 As shown, based on the changes in electrical signals, MXene thermoelectric fabrics can identify different breathing states of the body, such as normal breathing and deep breathing.
[0051] Therefore, the MXene thermoelectric fabric prepared by the present invention solves the problem of energy supply of wearable electronic devices themselves, can accurately monitor body breathing information under different states, and has potential application prospects in power generation, motion tracking and health monitoring.
[0052] Example 2
[0053] (1) a cotton fabric having a size of 1×20 cm was immersed in an ethanol solution having a volume concentration of 50% for 30 minutes, and then placed in a vacuum drying oven at 60° C. for 20 minutes to obtain a treated cotton fabric;
[0054] (2) placing the cotton fabric treated in step (1) into a 0.6% dopamine solution, adjusting the solution pH to 8.5, the reaction temperature to 35° C., shaking on a water bath shaker for 24 h, taking out and rinsing with deionized water to remove residues, and drying naturally at room temperature;
[0055] (3) immersing the cotton fabric obtained in step (2) in a chitosan solution having a mass concentration of 0.1% for 30 minutes to perform cationic modification on the cotton fabric to obtain a positively charged cotton fabric;
[0056] (4) First, 2 g LiF, 31 mL HCl (12 mol / L) and 9 mL deionized water were added to a polytetrafluoroethylene beaker, and the whole was placed in a water bath thermostat with a water bath temperature of 35 °C, a magnetic stirring speed of 400 rpm and a reaction time of 30 min. Then, 2 g Ti3AlC2 powder was slowly added to the mixed solution and the reaction lasted for 24 h at 35 °C. The obtained Ti3C2T x The product was washed with deionized water, each time at a centrifugal speed of 5000 rpm for 5 minutes, until the pH of the solution was close to neutral; then, deionized water was used as an intercalation agent, and the mixed solution was placed in an ultrasonic cleaning machine with a power of 500 W, and the ultrasonic cleaning was continued for 1 hour. Finally, the MXene dispersion was obtained by centrifugation at a speed of 5000 rpm for 5 minutes.
[0057] (5) The positively charged cotton fabric obtained in step (3) was placed in a 10 mg / mL MXene dispersion for 30 min, and then placed in a 50°C vacuum drying oven for 25 min to prepare a MXene thermoelectric fabric with cotton as the base material.
[0058] The MXene thermoelectric fabric prepared in Example 2 has an electrical conductivity of 221.6 S / m and a Seebeck coefficient of -8.92 μVK -1 , showing fast thermoelectric response capability and good thermoelectric stability; under a pressure of 250Pa, the air permeability of the MXene thermoelectric fabric prepared in Example 2 is 119mm / s.
[0059] Example 3
[0060] (1) placing a ketone-ammonia fabric having a size of 1×20 cm in an ethanol solution having a volume concentration of 40%, immersing the woven fabric for 30 min, taking the woven fabric out and placing the woven fabric in a vacuum drying oven at 60° C. for 20 min, thereby obtaining the treated ketone-ammonia fabric;
[0061] (2) placing the ketone-ammonia fabric treated in step (1) into a 0.8% dopamine solution, adjusting the solution pH to 8.5, the reaction temperature to 30° C., shaking on a water bath shaker for 12 h, taking out and rinsing the surface with deionized water to remove residues, and drying naturally at room temperature;
[0062] (3) immersing the ketone-ammonia fabric obtained in step (2) in a chitosan solution with a mass concentration of 1% for 30 minutes to perform cationic modification on the ketone-ammonia fabric to obtain a positively charged ketone-ammonia fabric;
[0063] (4) First, 2 g LiF, 31 mL HCl (12 mol / L) and 9 mL deionized water were added to a polytetrafluoroethylene beaker, and the whole was placed in a water bath thermostat with a water bath temperature of 35 °C, a magnetic stirring speed of 400 rpm and a reaction time of 30 min. Then, 2 g Ti3AlC2 powder was slowly added to the mixed solution and the reaction lasted for 24 h at 35 °C. The obtained Ti3C2T x The product was washed with deionized water, each time at a centrifugal speed of 5000 rpm for 5 minutes, until the pH of the solution was close to neutral; then, deionized water was used as an intercalation agent, and the mixed solution was placed in an ultrasonic cleaning machine with a power of 500 W, and the ultrasonic cleaning was continued for 1 hour. Finally, the MXene dispersion was obtained by centrifugation at a speed of 5000 rpm for 5 minutes.
[0064] (5) The positively charged ketone-amine fabric obtained in step (3) was placed in a 20 mg / mL MXene dispersion for 30 min, and then placed in a 50°C vacuum drying oven for 25 min to prepare a MXene thermoelectric fabric based on the ketone-amine fabric.
[0065] The MXene thermoelectric fabric prepared in Example 3 has an electrical conductivity of 269.6 S / m and a Seebeck coefficient of -8.14 μVK -1 , showing fast thermoelectric response capability and good thermoelectric stability; under a pressure of 250Pa, the air permeability of the MXene thermoelectric fabric prepared in Example 3 is 121mm / s.
[0066] Comparative Example 1
[0067] The preparation method of the MXene thermoelectric fabric of Comparative Example 1 is the same as that of Example 1, except that the nylon fabric is not soaked in chitosan solution. The specific preparation process is as follows:
[0068] (1) placing a 1×20 cm nylon fabric in an ethanol solution with a volume concentration of 50% for 30 minutes, taking it out and placing it in a 60° C. vacuum drying oven for 20 minutes to obtain a treated nylon fabric;
[0069] (2) placing the nylon fabric treated in step (1) into a 0.8% dopamine solution, adjusting the solution pH to 8.5, the reaction temperature to 35° C., shaking on a water bath shaker for 24 h, taking out and rinsing with deionized water to remove residues, and drying naturally at room temperature;
[0070] (3) First, 2 g LiF, 31 mL HCl (12 mol / L) and 9 mL deionized water were added to a polytetrafluoroethylene beaker, and the whole was placed in a water bath thermostat with a water bath temperature of 35 °C, a magnetic stirring speed of 400 rpm, and a reaction time of 30 min. Then, 2 g Ti3AlC2 powder was slowly added to the above mixed solution, and the reaction lasted for 24 h at 35 °C. The obtained Ti3C2T x The product was washed with deionized water, each time at a centrifugal speed of 5000 rpm for 5 minutes, until the pH of the solution was close to neutral. Afterwards, deionized water was used as an intercalation agent, and the mixed solution was placed in an ultrasonic cleaning machine with a power of 500 W for 1 hour. Finally, the mixture was centrifuged at a speed of 5000 rpm for 5 minutes to obtain a MXene solution.
[0071] (4) The nylon fabric obtained in step (2) was placed in a 15 mg / mL MXene dispersion for 30 min, and then placed in a 50°C vacuum drying oven for 25 min to prepare a MXene thermoelectric fabric.
[0072] The conductivity of the MXene thermoelectric fabric prepared in Comparative Example 1 is 231.6S / m, and the Seebeck coefficient is -9.9μVK -1 Compared with Example 1, the conductivity of the MXene thermoelectric fabric prepared in Comparative Example 1 is reduced and its Seebeck coefficient is reduced due to the lack of chitosan solution immersion treatment. Under a pressure of 250 Pa, the air permeability of the MXene thermoelectric fabric prepared in Comparative Example 1 is 135 mm / s.
[0073] Comparative Example 2
[0074] The preparation method of the MXene thermoelectric fabric of Comparative Example 2 is the same as that of Example 1, except that the nylon fabric is not modified with polydopamine. The specific preparation process is as follows:
[0075] (1) placing a 1×20 cm nylon fabric in an ethanol solution with a volume concentration of 50% for 30 minutes, taking it out and placing it in a 60° C. vacuum drying oven for 20 minutes to obtain a treated nylon fabric;
[0076] (2) immersing the nylon fabric obtained in step (1) in a chitosan solution having a mass concentration of 0.5% for 30 minutes to perform cationic modification on the nylon fabric to obtain a nylon fabric with a positive charge;
[0077] (3) The nylon fabric obtained in step (2) was placed in a 15 mg / mL MXene solution for 30 min, and then placed in a 50°C vacuum drying oven for 25 min to prepare a MXene thermoelectric fabric.
[0078] The conductivity of the MXene thermoelectric fabric prepared in Comparative Example 2 is 242.6S / m, and the Seebeck coefficient is -9.1μVK -1 Due to the lack of polydopamine modification, the conductivity of the MXene thermoelectric fabric prepared in Comparative Example 2 decreased and its Seebeck coefficient decreased compared with Example 1. Under a pressure of 250 Pa, the air permeability of the MXene thermoelectric fabric prepared in Comparative Example 2 was 134 mm / s.
[0079] Polydopamine modified fabric (Example 1) with a loading of 3 mg / cm2 at 15 mg / mL MXene dispersion 2 , fabric without polydopamine coating (Comparative Example 2), MXene loading at 1 mg / cm 2 .
[0080] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.
Claims
1. A method for preparing a stretchable MXene thermoelectric fabric, characterized in that: The steps include: (1) soaking the fabric in an ethanol solution and drying it to obtain a treated fabric; (2) placing the fabric treated in step (1) into a dopamine solution for reaction to obtain a polydopamine-modified fabric; (3) immersing the polydopamine-modified fabric obtained in step (2) in a chitosan solution to obtain a fabric with a positive charge; (4) Lithium fluoride, hydrochloric acid and deionized water are stirred and mixed to etch Ti3AlC2, the precipitate is separated and collected, the precipitate is dispersed using an intercalation agent, ultrasonically treated, and centrifuged to collect the upper MXene dispersion; (5) Immersing the positively charged fabric in step (3) in a MXene dispersion and drying to obtain a MXene thermoelectric fabric.
2. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (1), the fabric is one of nylon fabric, cotton fabric and ketone-ammonia fabric.
3. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (2), the mass concentration of the dopamine solution is 0.5-1%, and the pH value is 8-8.
5.
4. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (2), the reaction temperature is 25 to 40° C. and the reaction time is 8 to 24 hours.
5. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (3), the mass concentration of the chitosan solution is 0.1-1%; and the immersion time is 10-60 minutes.
6. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (4), the addition ratio of Ti3AlC2, lithium fluoride, hydrochloric acid and deionized water is 1g:1-1.5g:12-25mL:4.5mL; the etching temperature is 30-45°C, the etching time is 18-28h; and the concentration of hydrochloric acid is 12mol / L.
7. The method for preparing a stretchable MXene thermoelectric fabric according to claim 1, characterized in that: In step (5), the concentration of the MXene dispersion is 5 to 25 mg / mL.
8. The MXene thermoelectric fabric prepared by the method according to any one of claims 1 to 7.
9. Application of the MXene thermoelectric fabric described in claim 8 in the fields of power generation, sports tracking, and health monitoring.
10. A mask for human respiratory monitoring, characterized in that: The mask includes a mask body and a strap, and a MXene thermoelectric fabric sensor array is connected to the mask body. The specific preparation method is as follows: copper wire, conductive silver paste and copper tape are used to connect the MXene thermoelectric fabric described in claim 8 in series to obtain a MXene thermoelectric fabric sensor array; and then the MXene thermoelectric fabric sensor array is connected to the mask body by a flat needle method to obtain a mask for human breathing detection.
Citation Information
Patent Citations
Preparation method of polyaniline / MXene composite fabric and application of polyaniline / MXene composite fabric in printing and dyeing wastewater treatment
CN112064363A
Multilayer MXenes electromagnetic shielding fabric and preparation method thereof
CN113005780A
Flexible PPy / MXene-PDA photo-thermal fabric for solar evaporator and preparation method thereof
CN113882154A
Processing method of polyester fabric with photothermal effect
CN115679693A
Flexible electric heating fabric and preparation method thereof
CN115715083A