Silicon carbide-boron nitride gradient composite ceramic as well as preparation method and application thereof
Through the design of silicon carbide-boron nitride gradient composite ceramics, the gradient distribution of silicon carbide and the auxiliary-free low-pressure sintering process, the stability and preparation difficulty of boron nitride ceramics in high temperature environments are solved, and high mechanical properties are achieved and ceramic materials with stable high-temperature performance meet the complex use needs of side sealing plates.
Patent Information
- Application Number
- CN202411085881.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-08
AI Technical Summary
Existing boron nitride ceramics are prone to internal stress caused by temperature gradients in high-temperature environments, resulting in the breaking of the side sealing plate, and the residue of sintering additives and high sintering pressure increase the difficulty of the process, limiting its application.
Using silicon carbide-boron nitride gradient composite ceramic design, ceramic materials with high mechanical properties and stable high temperature properties are prepared through the gradient distribution of silicon carbide and the additive-free and low-pressure sintering process.
It realizes the simple and convenient preparation of boron nitride ceramics, improves Young's modulus and flexural strength, reduces the thermal expansion coefficient, meets the requirements of the complex use environment of the side sealing plate, and avoids the residue of sintering additives and high pressure. question.
Smart Images

Figure CN118930273A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of functional structural materials, and particularly relates to a silicon carbide-boron nitride gradient composite ceramic and a preparation method and application thereof. Background Art
[0002] Thin strip continuous casting technology is a new type of thin strip steel production process, which can directly obtain steel thin strips from high-temperature molten steel. Due to the elimination of hot rolling and other related processes in traditional continuous casting technology, the twin-roll thin strip continuous casting process requires a smaller site, a simpler process flow, greatly improved production efficiency, less equipment investment and low operating costs. It is one of the most advanced steelmaking technologies in the world. The side sealing plate can restrain the metal liquid, promote the forming of the thin strip, and ensure the edge quality of the thin strip. It is an important component of the twin-roll thin strip continuous casting process. It requires the material to have good thermal shock resistance, resistance to molten steel erosion, high temperature volume stability, non-wetting with molten steel and other characteristics as well as suitable wear resistance.
[0003] Hexagonal boron nitride is considered to be a very good candidate material for thin strip continuous casting side sealing plates due to its excellent high-temperature self-lubrication, good high-temperature resistance, high thermal conductivity, low thermal expansion coefficient, excellent insulation and easy processing. Although hexagonal boron nitride has many excellent properties, due to the strong covalent bond between the B and N atoms inside it, the solid phase diffusion is difficult, the melting point is high, and its own flaky structure makes it extremely difficult to sinter boron nitride ceramics to be dense, which greatly limits its application. In previous studies, the addition of sintering aids or the increase of sintering pressure were often used to promote and improve the sintering densification of boron nitride ceramics. For example, Zhai Fengrui et al. (Zhai Fengrui, Shan Ke, Lu Min, et al. Sintering and structure and properties of hexagonal boron nitride ceramics. Journal of the Chinese Ceramic Society, 2018, 46(6): 807-812) prepared h-BN ceramics by SPS sintering under the condition of adding B2O3 as a sintering aid. The results showed that the h-BN ceramics prepared by SPS had fine grains, high density, and a maximum flexural strength of 120 MPa. Baofo Qiu et al. (Qiu BF, Duan XM, Zhang Z, et al. Microstructural evolution and mechanical properties of h-BN composite ceramics with Y2O3-AlN addition by liquid-phase sintering. Rare Merals, 2020, 39(5): 555-561.) h-BN ceramics were prepared at 1800°C by hot pressing using Y2O3-AlN as a sintering aid. The maximum relative density and flexural strength (161 MPa) were obtained when the Y2O3-AlN addition was 40%. Although the addition of sintering aids will enhance the strength of boron nitride ceramics, the sintering aids will remain in the boron nitride ceramics as impurities, and the sintering aids generally have a low melting point. After addition, the high-temperature performance of boron nitride ceramics will be severely weakened. Increasing the sintering pressure can increase the relative density of boron nitride ceramics, but excessive sintering pressure will increase the difficulty of process implementation.
[0004] Since the side sealing plate needs to be in direct contact with the molten steel, the contact surface temperature can reach extremely high, about 1650°C, and there is a temperature difference of over 100 degrees with the interior. Once the internal stress generated by the temperature gradient is greater than the material strength, the side sealing plate will break, causing the side sealing plate to fail.
[0005] Therefore, how to design and provide a high-performance boron nitride ceramic material and a preparation method thereof to achieve simple and convenient preparation of the ceramic material and meet the requirements of the complex use environment of the side sealing plate is a key issue that scientific and technological personnel in this field urgently need to solve. Summary of the invention
[0006] In view of the defects of the prior art, the technical problem to be solved by the present invention is to provide a silicon carbide-boron nitride gradient composite ceramic and a preparation method and application thereof.
[0007] The invention provides a silicon carbide-boron nitride gradient composite ceramic, in which the silicon carbide content is distributed in a gradient manner.
[0008] The gradient composite ceramic is composed of boron nitride composite ceramics containing silicon carbide of different mass fractions distributed in layers.
[0009] The content of silicon carbide changes gradually from large to small or from small to large from the outer layer to the middle layer in the gradient ceramic.
[0010] The present invention provides a method for preparing a silicon carbide-boron nitride gradient composite ceramic, comprising:
[0011] (1) mixing silicon carbide and boron nitride according to a ratio to prepare silicon carbide and boron nitride composite powders with different ratios;
[0012] (2) Laying layers according to the gradient distribution of silicon carbide content and pre-pressing to obtain a ceramic body;
[0013] (3) The pre-pressed green body is pressurized and sintered in an inert atmosphere to obtain a silicon carbide-boron nitride gradient composite ceramic.
[0014] Preferably, in step (1), the boron nitride is composed of hexagonal boron nitride and cubic boron nitride, the hexagonal boron nitride accounts for 70-85% of the total boron nitride mass, and the cubic boron nitride accounts for 15-30%;
[0015] Preferably, in step (1), the average particle size of the silicon carbide powder is 100 nm or less; the average particle size of the hexagonal boron nitride is 1 μm or less, and the particle size of the cubic boron nitride is 500 nm or less.
[0016] The mixing method in step (1) is three-dimensional mixing, etc.
[0017] In step (2), powders of different proportions are spread layer by layer using a steel mold, and pre-pressed to obtain a ceramic body.
[0018] Preferably, the gradient distribution of the silicon carbide content in step (2) is that the silicon carbide content first increases gradually to the middle layer and then decreases gradually, or first decreases gradually to the middle layer and then increases gradually;
[0019] Preferably, the pre-pressing pressure in step (2) is 50 to 250 MPa.
[0020] Preferably, the inert atmosphere in step (3) is at least one of argon and nitrogen; the pressure sintering is hot pressing sintering or spark plasma sintering, wherein the sintering temperature is 1800-2000° C., the sintering pressure is 20-60 MPa, and the holding time is 5-100 min.
[0021] Preferably, in step (3), the silicon carbide-boron nitride gradient composite ceramic is provided with m layers; wherein the middle layer is the axis of symmetry, and the components and thicknesses of the axisymmetric layers are the same; wherein m≥3.
[0022] Preferably, the silicon carbide-boron nitride gradient composite ceramic consists of 5 layers, wherein the first layer and the fifth layer have the same powder composition, the second layer and the fourth layer have the same powder composition, and the third layer is an intermediate layer.
[0023] Preferably, m=5; wherein the silicon carbide content in the first and fifth layers of composite ceramics is 0-25wt.%, the silicon carbide content in the second and fourth layers of composite ceramics is 0-25wt.%, and the silicon carbide content in the third layer of composite ceramics is 0-25wt.%.
[0024] Preferably, m=5; wherein the thickness of the first and fifth layers accounts for 10-50% of the total thickness, the thickness of the second and fourth layers accounts for 10-50% of the total thickness, and the thickness of the third layer accounts for 10-50% of the total thickness.
[0025] The silicon carbide content in the silicon carbide-boron nitride gradient composite ceramic has a gradient distribution; wherein the silicon carbide content first increases gradually to the middle layer and then decreases gradually, or first decreases gradually to the middle layer and then increases gradually.
[0026] The component distribution index of the silicon carbide-boron nitride gradient composite ceramic is 0.8-1.2.
[0027] The present invention provides an application of the silicon carbide-boron nitride gradient composite ceramic in the field of thin strip continuous casting side sealing plate materials.
[0028] The present invention discloses a silicon carbide-boron nitride gradient composite ceramic and a preparation method thereof. The method introduces a silicon carbide second phase composite and designs a gradient ceramic. Without adding a sintering aid and applying a large sintering pressure, the method can realize a simple and convenient preparation of the boron nitride ceramic composite material, and at the same time can effectively improve its mechanical properties and ensure the high temperature performance of the boron nitride ceramic material, thereby meeting the requirements of the complex use environment of the side sealing plate.
[0029] Beneficial Effects
[0030] The present invention introduces silicon carbide as the second phase and performs gradient design to prepare silicon carbide-boron nitride gradient composite ceramics. This method does not require the addition of sintering aids and the application of large sintering pressure, and can achieve simple and convenient preparation. At the same time, the composite ceramic has a stronger Young's modulus and flexural strength and a lower thermal expansion coefficient. Since there is no sintering aid in the preparation process, the high-temperature performance of boron nitride ceramics is guaranteed. In addition, compared with traditional single-component boron nitride ceramics, the performance of the prepared gradient composite ceramics can be adjusted according to different application environments, thereby meeting more application scenarios and promoting the application and development of boron nitride materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 is a physical cross-sectional view of the sample with n=1.0 in Example 1 of the present invention;
[0032] Figure 2 are the bending and compressive strengths of each sample in Example 1 of the present invention;
[0033] Figure 3 is the Young's modulus of each sample in Example 1 of the present invention;
[0034] Figure 4 is the change of thermal expansion coefficient of each sample with temperature in Example 1 of the present invention;
[0035] Figure 5 is a physical cross-sectional view of the sample in Example 2 of the present invention;
[0036] Figure 6 It is a scanning electron microscope image of the sample in Example 2 of the present invention. DETAILED DESCRIPTION
[0037] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0038] Related tests:
[0039] The flexural strength and compressive strength of the samples were measured using a universal testing machine. The three-point flexural strength measurement required cutting the sample into four-sided strips with a cross-sectional length of 3×3 mm and a length of not less than 26 mm. The pressure loading rate was 0.05 mm / min, and the maximum load when the sample broke was recorded. The experiment was repeated at least 6 times for each sample.
[0040] For the measurement of compressive strength, the samples were cut into cubic prisms with a side length of 3±0.1 mm. The load loading rate was 0.1 mm / min, and the critical load borne by the test sample was recorded.
[0041] The hardness of the samples was measured using a Vickers hardness tester. The samples were tested after being ground and polished, and 5 data points were measured for each sample to obtain the average value.
[0042] The thermal diffusivity of h-BN in the direction parallel to the sintering pressure was measured using a laser thermal conductivity meter. The sample was a 10 mm diameter, 2 mm thick disc. After being polished, washed, dried, and sprayed with carbon powder, it was placed in a laser thermal conductivity meter to test the thermal diffusivity. Four temperature measurement points were selected: 30°C, 200°C, 400°C, and 600°C.
[0043] The thermal expansion coefficient of the sample was measured using a thermal expansion instrument. The sample was cut into a quadrangular prism with a cross-sectional side length of 3×3 mm and a length of 17 mm, and the surface of the sample was polished flat, with the angle between adjacent surfaces being 90°, and placed in a thermal expansion instrument to measure the thermal expansion coefficient.
[0044] raw material:
[0045]
[0046] Example 1
[0047] The powders are weighed according to the silicon carbide content of 0wt.% in the 1st and 5th layers of boron nitride powder, 5wt.% in the 2nd and 4th layers of boron nitride powder, and 10wt.% in the 3rd layer of boron nitride powder. In the above boron nitride powders, hexagonal boron nitride accounts for 70% of the total boron nitride, and cubic boron nitride accounts for 30% of the total boron nitride. A three-dimensional mixer is used to mix the powders, and the powders are spread out in a steel mold from 1 to 5 layers according to the thickness ratio in Table 1. A pressure of 150MPa is used to pre-press the laid powder to obtain a green body. The spark plasma sintering process is used, and the sintering is carried out at 2000℃ and 50MPa, and the holding time is 5min. The actual cross-section of the sample with n=1.0 is shown in the figure. Figure 1 shown.
[0048] like Figure 2 , 3 As shown in the figure, it can be seen that the flexural strength and Young's modulus of boron nitride ceramics are greatly improved by gradient design. With the increase of component distribution index n, the flexural strength shows a trend of first increasing and then decreasing. n = 1.0 has the maximum flexural strength (190 MPa), and the compressive strength of n = 1.2 reaches 286.3 MPa. The Young's modulus varies between 36.6 GPa and 39.62 GPa. Figure 4 The change of thermal expansion coefficient can be observed. It can be seen that the gradient design significantly reduces the thermal expansion coefficient of boron nitride ceramics at low temperature. The minimum thermal expansion coefficient can be reduced to 1.2×10 at 200°C. -6 K -1The thermal expansion coefficient of the prepared sample is between that of boron nitride ceramics containing 5% silicon carbide and that containing 10% silicon carbide, indicating that the gradient design can achieve the regulation of the thermal expansion coefficient of boron nitride ceramics by changing the thickness of the gradient layer.
[0049] Table 1
[0050]
[0051] Example 2
[0052] The powders are weighed according to the silicon carbide content of the first and fifth layers of boron nitride powder being 10wt.%, the silicon carbide content of the second and fourth layers of boron nitride powder being 5wt.%, and the silicon carbide content of the third layer of boron nitride powder being 0wt.%. In the above boron nitride powders, hexagonal boron nitride accounts for 80% of the total boron nitride, and cubic boron nitride accounts for 20% of the total boron nitride. A ball mill is used to mix the powders, and the powders are spread out in a steel mold from layer 1 to layer 5 according to the thickness ratio of n=1.0 in Table 1. A pressure of 200MPa is used to pre-press the laid powder to obtain a green body. A hot pressing sintering process is used, and sintering is carried out at 1900℃ and 50MPa, and the holding time is 50min. The actual cross-section of the sample is shown in the figure below. Figure 5 The microscopic morphology of the sample is shown in Figure 6 As shown in the figure, it can be seen that the grains of the samples obtained by hot pressing and sintering are larger, hexagonal, and the size is more than ten microns.
Claims
1. A silicon carbide-boron nitride gradient composite ceramic, characterized in that: The silicon carbide content in the silicon carbide-boron nitride gradient composite ceramic is distributed in a gradient manner.
2. A method for preparing a silicon carbide-boron nitride gradient composite ceramic, comprising: (1) mixing silicon carbide and boron nitride according to a ratio; (2) Laying layers according to the gradient distribution of silicon carbide content and pre-pressing to obtain a ceramic body; (3) Sintering under pressure in an inert atmosphere to obtain silicon carbide-boron nitride gradient composite ceramics.
3. The preparation method according to claim 2, characterized in that: In the step (1), the boron nitride is composed of hexagonal boron nitride and cubic boron nitride, wherein the hexagonal boron nitride accounts for 70-85% of the total boron nitride mass and the cubic boron nitride accounts for 15-30%; In step (1), the average particle size of the silicon carbide powder is less than 100 nm; the average particle size of the hexagonal boron nitride is less than 1 μm, and the particle size of the cubic boron nitride is less than 500 nm.
4. The preparation method according to claim 2, characterized in that: The gradient distribution of the silicon carbide content in the step (2) is that the silicon carbide content first increases gradually to the middle layer and then decreases gradually, or first decreases gradually to the middle layer and then increases gradually; the pre-pressing pressure is 50 to 250 MPa.
5. The preparation method according to claim 2, characterized in that: In the step (3), the inert atmosphere is at least one of argon and nitrogen; the pressure sintering is hot pressing sintering or spark plasma sintering, wherein the sintering temperature is 1800-2000° C., the sintering pressure is 20-60 MPa, and the holding time is 5-100 min.
6. The preparation method according to claim 2, characterized in that: In the step (3), the silicon carbide-boron nitride gradient composite ceramic is provided with m layers, wherein m≥3; wherein the middle layer is the symmetry axis, and the components and thicknesses of the axisymmetric layers are the same.
7. The preparation method according to claim 6, characterized in that: The silicon carbide-boron nitride gradient composite ceramic consists of five layers, wherein the first layer has the same composition as the fifth layer, the second layer has the same composition as the fourth layer, and the third layer is an intermediate layer.
8. The preparation method according to claim 6, characterized in that: The m=5; wherein the silicon carbide content in the first and fifth layers of the composite ceramic is 0-25wt.%, the silicon carbide content in the second and fourth layers of the composite ceramic is 0-25wt.%, and the silicon carbide content in the third layer of the composite ceramic is 0-25wt.%.
9. The preparation method according to claim 6, characterized in that: The m=5; wherein the thickness of the first and fifth layers accounts for 10-50% of the total thickness, the thickness of the second and fourth layers accounts for 10-50% of the total thickness, and the thickness of the third layer accounts for 10-50% of the total thickness.
10. An application of the silicon carbide-boron nitride gradient composite ceramic according to claim 1 in the field of thin strip continuous casting side sealing plate materials.
Citation Information
Patent Citations
Method for preparing SiC / BN layered composite ceramic
CN101134674A
Preparation method of layered structure ceramic ring for mechanical sealing
CN111825454A
Composite side sealing plate and preparation method thereof
CN117600422A
Ceramic composite body used in the production of bearing bushings, bearing shafts, nozzles, sliding bearings or sliding ring seals comprises an outer casing ceramic and a sintered material having electrical and / or mechanical properties
DE10141660A1
Improved silicon carbide composite and process for production
EP0056596A1
Cited By
Preparation method and application of silicon carbide ceramic combined aluminum silicon carbide gradient material
CN121159257A