Sintering process of high-strength injection-molded zirconia ceramic

By coupling the nanozirconia powder and using the high and low temperature composite two-stage sintering process, the problems of agglomeration and sintering temperature sensitivity of nanozirconia powder are solved, and the high strength and uniform microstructure of zirconia ceramics are achieved, improving the Its density and bending strength are achieved.

CN118930289APending Publication Date: 2024-11-12ZHEJIANG UNIV OF TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410981577.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The high surface energy of nanozirconia powder causes powder agglomeration, affecting the uniform dispersion and sintering performance during injection molding, resulting in the sintering temperature being sensitive to grain growth, making it difficult to densify at low temperatures and abnormal grain growth at high temperatures. The strength of zirconia ceramics is limited.

Method used

The nanozirconia powder is coupled with the coupling agent and injection molded with the composite adhesive. The high and low temperature composite two-stage sintering process is adopted to eliminate the air holes by rapidly increasing the temperature and extend the sintering time to form a uniform microstructure. .

Benefits of technology

It effectively improves the density and bending strength of zirconia ceramics, inhibits abnormal grain growth, and improves the densification and mechanical properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930289A_ABST
    Figure CN118930289A_ABST
Patent Text Reader

Abstract

The invention discloses a sintering process of high-strength injection-molded zirconia ceramic. The preparation method comprises the following steps: by taking nano zirconium oxide powder as a raw material, adding a coupling agent, mixing, stirring and drying to obtain modified zirconium oxide powder, carrying out injection molding to obtain a green body, degreasing, and carrying out high-low temperature composite two-stage sintering in air to obtain the high-strength injection-molded zirconium oxide ceramic. According to the invention, nano zirconia powder is modified by a coupling agent, a two-stage sintering process is cooperated and compounded, an injection molded blank is heated to a high temperature within a short time, zirconia ceramic is subjected to first-stage sintering and rapid densification, and then the sintering temperature is reduced to a low temperature for long-time sintering, so that the high-density zirconia ceramic is obtained. The abnormal growth of the crystal grains is inhibited, the microstructure uniformity of the material is kept, and the bending strength of the final ceramic body is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic injection molding, and in particular relates to a sintering process for injection-molded zirconia ceramics. Background Art

[0002] Ceramic injection molding (CIM) is a process for powder metallurgy molding of ceramic powders, involving four main processes: mixing, injection, degreasing and sintering. This process has the advantages of wide application of materials, preparation of complex-shaped parts, high degree of production automation and high product stability.

[0003] Smaller nano-zirconia powders are usually used as raw materials for the preparation of zirconia ceramics. However, the high surface energy of nano-powders causes powder agglomeration, which has a great influence on the injection molding process. In order to obtain higher powder filling amount, good flow properties and sintering performance, the surface of zirconia powders needs to be modified. In addition, when the particle size of zirconia raw materials is small, the sintering speed is fast and more difficult to control. When the sintering temperature is low, the grain growth is incomplete and the sintering is insufficient, which affects its strength. When the sintering temperature is too high, abnormal grain growth is likely to occur, which also leads to a decrease in strength. This is the main problem that limits the improvement of the strength of injection-molded zirconia ceramics.

[0004] Nano-zirconia powder can be sintered to a high density at a relatively low temperature and without sintering additives due to its high sintering activity. However, due to the high surface energy and strong activity of nano-zirconia powder, particles are prone to agglomeration, which affects the uniform dispersion and fluidity of the powder in injection molding and the grain growth during sintering. For nano-zirconia powder, the sintering temperature has an important influence on its grain growth. If the sintering temperature is too low, the densification is insufficient, which will lead to a decrease in density and bending strength. On the contrary, if the sintering temperature is too high, the grains will grow abnormally and the bending strength will also decrease. In addition, even at a relatively low sintering temperature (such as 1500°C), abnormal grain growth is found. Therefore, in order to solve the problem that nano-zirconia powder is easy to agglomerate, resulting in difficulty in sintering and low strength, the present invention couples the zirconia powder and coordinates the composite two-stage sintering process to control the sintering densification and grain growth process of injection molded zirconia ceramics, thereby improving its mechanical properties. Summary of the invention

[0005] The purpose of the present invention is to provide a sintering process for high-strength injection-molded zirconia ceramics in view of the deficiencies in the prior art.

[0006] The present invention adopts the following technical solutions:

[0007] Step (1), using a coupling agent to couple the nano zirconium oxide powder to obtain modified zirconium oxide powder;

[0008] Preferably, the nano zirconium oxide powder is yttria-stabilized zirconium oxide (3Y-TZP) powder, and the particle size is 50 to 100 nm;

[0009] Preferably, the coupling agent is a silane coupling agent or a zirconate coupling agent, and more preferably a zirconate coupling agent. The mass ratio of the coupling agent to the nano zirconium oxide powder is (0.2-1.0):100.

[0010] Step (2), mixing the modified zirconia powder obtained in step (1) with a composite binder, and injection molding to obtain a zirconia blank;

[0011] Preferably, the composite binder comprises polyethylene and paraffin in a mass ratio of (50-60): (40-50);

[0012] Preferably, the mass ratio of the zirconium oxide powder to the composite binder is (86-88):(14-12).

[0013] Step (3), after degreasing the zirconia blank obtained in step (2), sintering it in air through a high-low temperature composite two-stage sintering to obtain a high-strength injection-molded zirconia ceramic.

[0014] The composite two-stage sintering process is to heat to 1550-1600°C at a heating rate of 5-10°C / min, sinter for 5-120s; then cool to 1300-1450°C, and sinter for 4-10h; preferably, heat to 1575°C at a heating rate of 5°C / min, sinter for 60s; then cool to 1400°C, and sinter for 8h.

[0015] Compared with the prior art, the present invention has the following advantages:

[0016] The present invention effectively improves the dispersion of zirconium oxide powder by adding a coupling agent, reduces particle agglomeration, and increases the fluidity of injection molding granular materials, thereby improving the uniformity and consistency of the injection molding blank, reducing the defects of the blank and the later sintered body; at the same time, the uniformly dispersed nano zirconium oxide particles will form a better microstructure during the sintering process. In addition, the composite two-stage sintering process is also coordinated. By raising the injection molding blank to a higher temperature (1550-1600°C) in a shorter time, the pores can be quickly eliminated, the densification process can be improved, and the zirconium oxide ceramics can be quickly densified by the first stage sintering, and then the sintering temperature is reduced to a lower temperature (1300-1450°C) for a long time sintering, so that the grain growth is complete and the abnormal growth of the grains is suppressed, thereby obtaining fine and uniform grains, which helps to improve the bending strength of the final material. At the same time, the composite two-stage sintering process can suppress the abnormal growth of the grains and the appearance of abnormally large grains, thereby maintaining the uniformity of the microstructure of the material, which also improves the bending strength of the final ceramic body.

[0017] In summary, the method of the present invention can effectively improve the microstructure of injection-molded zirconia ceramics and increase the density and bending strength of ceramic materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a scanning electron microscope image of the cross section of the sintered sample obtained in Example 1.

[0019] Figure 2 This is a scanning electron microscope image of the cross section of the sintered sample obtained in Example 3.

[0020] Figure 3 This is a scanning electron microscope image of the cross section of the sintered sample obtained in Comparative Example 1. DETAILED DESCRIPTION

[0021] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0022] Example 1

[0023] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 0.2wt% of zirconate coupling agent (C 26 H 44 O 16 Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (the mass ratio of polyethylene to paraffin is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at a temperature of 145°C and a pressure of 70MPa to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1575°C at a heating rate of 5°C / min and sintered for 60s; then cooled to 1400°C and sintered for 8h to finally obtain a high-strength zirconia ceramic sintered body. The micromorphology of the obtained product was observed and measured by scanning electron microscopy, three-point bending method and drainage method, as well as its bending strength and density. As shown in the attached figure Figure 1 As shown, the grains on the cross section of the zirconia sintered body grow evenly without defects such as holes and cracks. The grain size, density and bending strength are shown in Table 1.

[0024] Example 2

[0025] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and couple it with a silane coupling agent (KH151) accounting for 0.5wt% of the mass of the zirconium oxide powder to obtain a modified zirconium oxide powder. Then, 224g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 50:50) is mixed with 1500g of modified zirconium oxide powder to obtain injection molding feed. Using an injection molding machine, the feed is injection molded at 145℃ and 70MPa to obtain a rectangular body with a size of 80mm×10mm×4mm. After degreasing the body, it is heated to 1600℃ at a heating rate of 10℃ / min and sintered for 5s; then cooled to 1450℃ and sintered for 4h to finally obtain a high-strength zirconium oxide ceramic sintered body. The flexural strength and density are measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0026] Example 3

[0027] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 1.0wt% of zirconate coupling agent (C 26 H 44 O 16 Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 204.5g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 50:50) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at a temperature of 145°C and a pressure of 70MPa to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1550°C at a heating rate of 5°C / min and sintered for 60s; then cooled to 1300°C and sintered for 10h to finally obtain a high-strength zirconia ceramic sintered body. The micromorphology of the obtained product was observed and measured by scanning electron microscopy, three-point bending method and drainage method, as well as its bending strength and density. As shown in the attached Figure 2 As shown, the grains on the cross section of the zirconia sintered body grow evenly without defects such as holes and cracks. The grain size, density and bending strength are shown in Table 1.

[0028] Example 4

[0029] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 0.5wt% of zirconate coupling agent (C 26 H 44 O 16Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa pressure to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1550℃ at a heating rate of 10℃ / min and sintered for 120s; then cooled to 1400℃ and sintered for 10h to finally obtain a high-strength zirconia ceramic sintered body. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0030] Example 5

[0031] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 0.5wt% of zirconate coupling agent (C 26 H 44 O 16 Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa pressure to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1600℃ at a heating rate of 5℃ / min and sintered for 60s; then cooled to 1300℃ and sintered for 4h to finally obtain a high-strength zirconia ceramic sintered body. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0032] Example 6

[0033] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 1.0wt% of zirconate coupling agent (C 26 H 44 O 16Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding material. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa pressure to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1600℃ at a heating rate of 5℃ / min and sintered for 60s; then cooled to 1450℃ and sintered for 4h to finally obtain a high-strength zirconia ceramic sintered body. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0034] Comparative Example 1 (conventional sintering without adding coupling agent)

[0035] First, weigh 1500g of nano-zirconia powder (50-100nm) into a beaker, and then mix 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) with 1500g of zirconium oxide powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1575℃ at a heating rate of 5℃ / min and sintered for 4h to finally obtain a zirconia ceramic sintered body. The micromorphology of the obtained product was observed by scanning electron microscopy, three-point bending method and drainage method, and its bending strength and density were tested. As shown in the attached figure Figure 3 As shown in Table 1, the grain growth and distribution on the cross section of the zirconia sintered body are uneven, and abnormal grain growth occurs. The grain size, density and bending strength of the sintered body are shown in Table 1.

[0036] Comparative Example 2 (Conventional sintering with addition of coupling agent)

[0037] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 0.2wt% of zirconate coupling agent (C 26 H 44 O 16 Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa pressure to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1575℃ at a heating rate of 5℃ / min and sintered for 4h. Finally, a zirconia ceramic sintered body was obtained. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0038] Comparative Example 3 (adding coupling agent and sintering in one step)

[0039] First, weigh 1500g of nano zirconium oxide powder (50-100nm) in a beaker, and use 0.2wt% of zirconate coupling agent (C 26 H 44 O 16 Zr) was subjected to coupling treatment to obtain modified zirconia powder. Then 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio is 60:40) was mixed with 1500g of modified zirconia powder to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa pressure to obtain a rectangular green body with a size of 80mm×10mm×4mm. After degreasing the green body, it was heated to 1575℃ at a heating rate of 5℃ / min and sintered for 60s. Finally, a zirconia ceramic sintered body was obtained. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0040] Comparative Example 4 (composite two-stage sintering without adding coupling agent)

[0041] 244g of polyethylene / paraffin composite binder (polyethylene, paraffin mass ratio of 60:40) was mixed with 1500g of nano zirconium oxide powder (50-100nm) to obtain injection molding feed. Using an injection molding machine, the feed was injection molded at 145℃ and 70MPa to obtain a rectangular body with a size of 80mm×10mm×4mm. After degreasing the body, it was heated to 1575℃ at a heating rate of 5℃ / min and sintered for 60s; then cooled to 1400℃ and sintered for 8h. Finally, a zirconia ceramic sintered body was obtained. The flexural strength and density were measured by the three-point bending method and the drainage method. The grain size, density and flexural strength of the sintered body are shown in Table 1.

[0042] The unmodified nano-zirconia powder is more prone to abnormal grain growth during the sintering process, resulting in a decrease in the density and mechanical properties of the material. However, due to the barrier of the coupling layer, the grain growth of the coupled modified nano-zirconia powder is more uniform during sintering, and the abnormal grain growth is suppressed.

[0043] Table 1: Grain size, density and flexural strength of sintered bodies of Examples and Comparative Examples.

[0044]

[0045] It can be seen from Table 1 that due to the use of nano zirconium oxide powder, the density of the sintered body is not much different in both the embodiment and the comparative example under the sintering conditions, and is in the range of 6.01 to 6.03 g / cm 3The densification degree is high. However, under conventional sintering conditions, the grain size of the sintered body increases significantly with the increase of sintering time, and the bending strength is low. The bending strength of the sintered body after coupling modification and high and low temperature two-stage sintering is greatly improved. In the case of the obtained injection molding specimen, the bending strength of the sintered body is much greater than the bending strength of the samples without coupling (Comparative Example 1), simple coupling (Comparative Example 2) or simple two-stage sintering (Comparative Example 4), and can even reach 577MPa.

Claims

1. A sintering process for high-strength injection-molded zirconia ceramics, characterized in that: The steps include: Step (1), using a coupling agent to couple the nano zirconium oxide powder to obtain modified zirconium oxide powder; Step (2), mixing the modified zirconia powder obtained in step (1) with a composite binder, and injection molding to obtain a zirconia blank; Step (3), after degreasing the zirconia blank obtained in step (2), sintering it in air in two stages at high and low temperatures to obtain a high-strength injection-molded zirconia ceramic; The composite two-stage sintering process is to heat to 1550-1600° C. at a heating rate of 5-10° C. / min, sinter for 5-120 seconds, and then cool to 1300-1450° C., and sinter for 4-10 hours.

2. The process according to claim 1, characterized in that The particle size of the nano zirconium oxide powder is 50-100 nm.

3. The process according to claim 1, characterized in that The coupling agent is a silane coupling agent or a zirconate coupling agent.

4. The process according to claim 3, characterized in that The coupling agent is a zirconate coupling agent.

5. The process according to claim 1, characterized in that The mass ratio of the coupling agent to the nano zirconium oxide powder is (0.2-1.0):

100.

6. The process according to claim 1, characterized in that The composite adhesive comprises polyethylene and paraffin in a mass ratio of (50-60):(40-50).

7. The process according to claim 1, characterized in that The mass ratio of the modified zirconium oxide powder to the binder is (86-88): (14-12).

8. The process according to claim 1, characterized in that Preferably, the temperature is heated to 1575°C at a heating rate of 5°C / min and sintered for 60s; Then cool down to 1400℃ and sinter for 8h.

9. A high-strength injection-molded zirconia ceramic prepared by the process according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Firing method of ultrafine-grained zirconia ceramic

    CN103396118A

  • Manufacturing method and application of alveolate blind hole toughened zirconium oxide ceramic shell

    CN107573061A

  • Feed material for injection molding of nano zirconium-based ceramic as well as preparation method and application of feed material

    CN116082037A

  • Method for preparing transparent ceramic part by injection molding

    WO2017133049A1