Method for preparing material for absorbing, storing and slowly releasing water and fertilizer by using desulfurized gypsum

By mixing desulfurization gypsum, fly ash, clay waste and other materials in a specific proportion and firing at high temperature, water-absorbing materials that are resistant to salt, alkali, high temperature and ultraviolet rays are prepared, which solves the volume expansion and water absorption rate reduction after water absorption of the water retention agent is solved. The problem of this achieves rapid and repeated water absorption and soil structure protection.

CN118930313APending Publication Date: 2024-11-12GANSU HAOYUAN HENGXIN TECHNOLOGY DEVELOPMENT CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411235112.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing water retention agent expands greatly after absorbing water, destroying the soil structure and affecting plant growth. The water absorption rate is slow. After multiple water absorption, the water absorption rate rapidly decays, and is not resistant to saline, alkali, high temperature, and ultraviolet rays, resulting in soil crumbing.

Method used

Desulfurization gypsum, fly ash, clay waste, binder and hot melt are mixed in a specific proportion, and after grinding, grinding, granulation, drying and high temperature firing, non-ceramic granular materials with open pore structure are prepared.

Benefits of technology

The volume of this material remains unchanged before and after water absorption, and its water absorption capacity does not decrease after multiple times. It absorbs water quickly, is resistant to saline, alkali, high temperature, and ultraviolet rays, and maintains good soil structure and water absorption performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930313A_ABST
    Figure CN118930313A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of industrial solid waste resource utilization and novel environment-friendly material preparation, in particular to a method for preparing a material for absorbing, storing and slowly releasing water and fertilizer by utilizing desulfurized gypsum. The invention relates to a method for preparing a material for absorbing, storing and slowly releasing water and fertilizer by using desulfurized gypsum. The method comprises the following steps: step 1, preparing raw materials; step 2, mixing the raw materials; step 3, granulating the raw materials; the product provided by the invention has good water absorption, the volume is not changed before and after water absorption, and the soil structure is not influenced; after multiple times of water absorption, the repeated water absorption capacity is not reduced; the water absorption speed is high, the water absorption capacity is not affected by ions and soil components, and saline-alkali resistance, high temperature, ultraviolet rays and the like are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial solid waste resource utilization and new environmentally friendly material preparation, and specifically to a method for preparing a water-fertilizer storage and slow-release material by utilizing desulfurized gypsum. Background Art

[0002] Super absorbent resin is a functional polymer material containing strong hydrophilic groups and a certain degree of crosslinking. It is widely used in medical and health care, building materials, environmental protection, agriculture, forestry and food industry. For example, it is used in diapers, sanitary napkins, napkins, and can also be used as a thickener for cosmetics, ointments, drugs, detergents, soil improvers, drug sustained-release bases, cement, mortar, concrete modifiers, afforestation seedling water-retaining agents, etc. In my country, super absorbent resins used in agriculture and forestry are generally referred to as water-retaining agents.

[0003] After decades of application practice, the application of water retaining agents in agriculture and forestry has verified the value of water retaining materials, but water retaining agents have obvious disadvantages. After absorbing water, the volume expands greatly, which destroys the soil structure and causes poor soil permeability, affecting plant growth; after absorbing water many times, the water absorption rate decays rapidly or even loses the ability to absorb water; most water retaining agent products absorb water slowly, which takes about 30 minutes or more, and cannot effectively absorb and utilize rainwater; the water absorption rate is greatly affected by cations and soil components, and is not resistant to salinity, high temperature, ultraviolet rays, etc., and causes soil compaction. Summary of the invention

[0004] In view of the existing problems, the present invention provides a method for preparing a water-fertilizer storage and slow-release material using desulfurized gypsum to solve the obvious drawbacks of the water-retaining agent mentioned in the background technology. The volume of the water-retaining agent greatly expands after absorbing water, destroying the soil structure and causing poor soil permeability, affecting plant growth; after absorbing water many times, the water absorption rate decays rapidly or even loses the water absorption capacity; most water-retaining agent products absorb water slowly, which takes about 30 minutes or more, and cannot effectively absorb and utilize rainwater; the water absorption rate is greatly affected by cations and soil components, and is not resistant to salt, alkali, high temperature, ultraviolet rays, etc., and causes the problem of soil compaction.

[0005] In order to solve the existing problems, the present invention provides a method for preparing a water-fertilizer storage and slow-release material using desulfurized gypsum, comprising step one: preparing raw materials, step two: mixing raw materials, step three: granulating raw materials, step four: drying particles, and step five: high-temperature calcining particles;

[0006] The step 1: raw material preparation includes grinding the raw materials to make the raw material particle size within the range of 100 to 200 meshes;

[0007] Step 2: The raw materials are mixed in a mass ratio of: 10% to 60% desulfurized gypsum, 20% to 30% fly ash, 40% to 70% clay waste, 2% adhesive, 5% to 10% hot melt, weighed in proportion, put into a powder mixer and mixed evenly, and about 7% of water is added to continue stirring evenly;

[0008] The step 3: granulating the raw materials is to granulate the raw materials evenly stirred in the step 2 in a granulator to form oblate particles of uniform size;

[0009] The fourth step: drying the particles is to place the particles prepared in the third step into a hot air dryer and dry them at 120° C. to a state where the moisture content is less than 3%.

[0010] The step five: high temperature sintering of particles is to feed the particles dried in the step four into a rotary tube kiln, raise the temperature to 800-1100° C., and calcine for about 30 minutes to obtain product particles.

[0011] Furthermore, the internal structure of the product particles is open pores and is made of non-ceramic material.

[0012] Furthermore, the diameter of the product particles is about 9 mm.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] 1. The product particles of the present invention have good water absorption, and the volume remains unchanged before and after water absorption, and does not affect the soil structure; after multiple water absorption, the repeated water absorption capacity does not decrease; the water absorption speed is fast; the water absorption capacity is not affected by ions and soil components, and is resistant to salt, alkali, high temperature, ultraviolet rays, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The process flow chart of the present invention is DETAILED DESCRIPTION

[0016] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0017] refer to Figure 1 , a method for preparing water-fertilizer storage and slow-release materials using desulfurized gypsum, comprising step one: raw material preparation, step two: raw material mixing, step three: raw material granulation, step four: granule drying, step five: granule high temperature firing;

[0018] The step 1: raw material preparation includes grinding the raw materials to make the raw material particle size within the range of 100 to 200 meshes;

[0019] Step 2: The raw materials are mixed in a mass ratio of: 10% to 60% desulfurized gypsum, 20% to 30% fly ash, 40% to 70% clay waste, 2% adhesive, 5% to 10% hot melt, weighed in proportion, put into a powder mixer and mixed evenly, and about 7% of water is added to continue stirring evenly;

[0020] The step 3: granulating the raw materials is to granulate the raw materials evenly stirred in the step 2 in a granulator to form oblate particles of uniform size;

[0021] The fourth step: drying the particles is to place the particles prepared in the third step into a hot air dryer and dry them at 120° C. to a state where the moisture content is less than 3%.

[0022] The step five: high temperature sintering of particles is to feed the particles dried in the step four into a rotary tube kiln, raise the temperature to 800-1100° C., and calcine for about 30 minutes to obtain product particles.

[0023] It should be noted that the clay waste can be one of sand washing mud, sludge, and construction waste; the adhesive can be carboxymethyl cellulose or calcium lignin sulfonate; and the hot melt can be coal gangue or feldspar.

[0024] The internal structure of the product particles is open pores and is made of non-ceramic material.

[0025] Wherein, the diameter of the product particles is about 9 mm.

[0026] Embodiment 1: During production, the raw materials are first prepared, and the desulfurized gypsum, fly ash, and clay waste are respectively put into a grinder for grinding, and the particle fineness of the desulfurized gypsum, fly ash, and clay waste is controlled at 100 mesh; then, according to the mass ratio: 30% of desulfurized gypsum, 20% of fly ash, 40% of clay waste, 2% of adhesive, and 8% of hot melt are weighed respectively, and the raw materials weighed according to the mass ratio are put into a mixer and stirred and mixed evenly, and then about 7% of water is added to continue stirring evenly, and then the mixed raw materials are put into a granulator for granulation to form oblate particles of uniform size, and the prepared particles are put into a hot air dryer, and dried at 120°C to a moisture content of less than 3%, and then the dried particles are transferred to a rotary pipeline kiln and heated to 800°C, and fired for about 30 minutes to obtain product particles.

[0027] Embodiment 2: During production, the raw materials are first prepared, and the desulfurized gypsum, fly ash, and clay waste are respectively put into a grinder for grinding, and the particle fineness of the desulfurized gypsum, fly ash, and clay waste is controlled at 150 mesh; then, according to the mass ratio: 40% of desulfurized gypsum, 25% of fly ash, 50% of clay waste, 2% of adhesive, and 7% of hot melt are weighed respectively, and the above raw materials weighed according to the mass ratio are put into a mixer and stirred and mixed evenly, and then about 7% of water is added to continue stirring evenly, and then the mixed raw materials are put into a granulator for granulation to form oblate particles of uniform size, and the prepared particles are put into a hot air dryer, and dried at 120°C to a moisture content of less than 3%, and then the dried particles are transferred to a rotary pipeline kiln and heated to 900°C, and fired for about 30 minutes to obtain product particles.

[0028] Embodiment 3: During production, the raw materials are first prepared, and the desulfurized gypsum, fly ash, and clay waste are respectively put into a grinder for grinding, and the particle fineness of the desulfurized gypsum, fly ash, and clay waste is controlled at 200 mesh; then, they are weighed according to the mass ratio: 58% of desulfurized gypsum, 28% of fly ash, 69% of clay waste, 2% of adhesive, and 9% of hot melt, and the raw materials weighed according to the mass ratio are put into a mixer and stirred and mixed evenly, and then about 7% of water is added to continue stirring evenly, and then the mixed raw materials are put into a granulator for granulation to form oblate particles of uniform size, and the prepared particles are put into a hot air dryer and dried at 120°C to a moisture content of less than 3%, and then the dried particles are transferred to a rotary pipeline kiln and heated to 1100°C, and fired for about 30 minutes to obtain product particles.

[0029] The volume of the product particles obtained in Examples 1 to 3 remains unchanged after absorbing water. A product with a volume of 1 liter can absorb and store about 0.5 liters of tap water or irrigation water or a water-fertilizer mixed solution. When used for desert transformation in production practice, sand and the product can be mixed in a volume ratio of 1:1. After the mixture is irrigated with water, it can maintain a water content of 25% by volume, which has a good soil moisture content.

[0030] The water absorption rate is fast. This product can quickly absorb a large amount of water. It can absorb more than 90% of its maximum water absorption capacity within 10 seconds. It can quickly absorb and store water for plant growth on rainy days.

[0031] The product has strong ability to absorb water repeatedly. After absorbing tap water for more than 20 times, its water absorption rate can still be maintained or even slightly improved. Compared with organic water retaining agents, after absorbing tap water for more than 5 times, its water absorption rate will generally drop to about 20% of the initial value. If it absorbs tap water for more than 20 times, its water absorption rate will be reduced to close to 0, which is equivalent to failure.

[0032] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. The replacement may be a replacement of a part of the structure, device, method step, or a complete technical solution. Any equivalent replacement or change according to the technical solution and the inventive concept of the present invention shall be covered within the protection scope of the present invention.

Claims

1. A method for preparing a water-fertilizer storage and slow-release material using desulfurized gypsum, characterized in that: The method comprises the steps of: preparing raw materials, mixing raw materials, granulating raw materials, drying granules, and sintering granules at high temperature; The step 1: raw material preparation includes grinding the raw materials to make the raw material particle size within the range of 100 to 200 meshes; Step 2: The raw materials are mixed in a mass ratio of: 10% to 60% desulfurized gypsum, 20% to 30% fly ash, 40% to 70% clay waste, 2% adhesive, 5% to 10% hot melt, weighed in proportion, put into a powder mixer and mixed evenly, and about 7% of water is added to continue stirring evenly; The step 3: granulating the raw materials is to granulate the raw materials evenly stirred in the step 2 in a granulator to form oblate particles of uniform size; The fourth step: drying the particles is to place the particles prepared in the third step into a hot air dryer and dry them at 120° C. to a state where the moisture content is less than 3%. The step five: high temperature sintering of particles is to feed the particles dried in the step four into a rotary tube kiln, raise the temperature to 800-1100° C., and calcine for about 30 minutes to obtain product particles.

2. The method for preparing water-fertilizer storage and slow-release material using desulfurized gypsum according to claim 1, characterized in that: The internal structure of the product particles is open pores and is made of non-ceramic material.

3. The method for preparing water-fertilizer storage and slow-release material using desulfurized gypsum according to claim 1, characterized in that: The diameter of the product particles is about 9 mm.

Citation Information

Patent Citations

  • Desulfurized gypsum light through-pore ceramsite

    CN106083156A

  • Desulfurized gypsum granular soil and preparation method thereof

    CN110964531A

  • Industrial, agricultural and urban solid waste-based ceramsite as well as preparation method and application thereof

    CN114804910A