Porous ceramic, preparation method thereof and atomizing core

By using the combination of raw materials such as skeleton materials, boron oxide, illite and glass microbeads, combined with mechanical ball milling and dry press forming processes, the problem of insufficient strength of porous ceramics is solved, significantly improving the strength and stability of the ceramics and reducing atomization The assembly failure of the core extends its service life.

CN118930315APending Publication Date: 2024-11-12SHENZHEN JIJIA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411013469.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The strength of existing porous ceramics is poor, which causes the atomized core to be easily damaged or powdered during assembly, affecting its life and safety.

Method used

The porous ceramics are prepared by mechanical ball milling, dry press molding and sintering processes by adjusting the raw material and sintering ratio and sintering conditions to improve the strength and chemical stability of the ceramics.

Benefits of technology

It significantly improves the strength and earthquake resistance of porous ceramics, reduces the damage and powder loss of the ceramic substrate during assembly, extends the service life of the atomized core and improves safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004965992920000091
    Figure BDA0004965992920000091
  • Figure BDA0004965992920000101
    Figure BDA0004965992920000101
Patent Text Reader

Abstract

The invention belongs to the technical field of porous ceramic preparation, and relates to a porous ceramic, a preparation method thereof and an atomizing core, and the porous ceramic comprises the following raw materials: a framework material, boric oxide, illite, a glass material and hollow glass beads. In the technical scheme provided by the invention, the illite can obviously reduce the sintering temperature under the activation action of the boric oxide, and meanwhile, the strength, chemical stability and thermal stability of the porous ceramic can be improved; the atomizing core is prepared from the porous ceramic, so that the strength and shock resistance of the atomizing core can be improved, and the phenomena that the ceramic matrix is easy to damage and powder falls off when the atomizing core is assembled are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of porous ceramic preparation, and in particular to a porous ceramic, a preparation method thereof, and an atomizing core. Background Art

[0002] Porous ceramics have the characteristics of porous structure, strong lipophilicity, uniform heat generation, and high temperature resistance, and are good raw materials for the preparation of atomizer cores. In the prior art, the traditional preparation process of porous ceramics is to use diatomaceous earth as the main matrix material, and add a binder and a pore-forming agent for sintering.

[0003] However, the silica contained in diatomaceous earth is amorphous silica, and the strength increased by crystal transformation during high-temperature sintering is limited, which makes the strength of porous ceramics poor. The atomizer core made of porous ceramics is prone to breakage or even powder loss during assembly, affecting the life and safety of the atomizer core. Summary of the invention

[0004] The purpose of the embodiments of the present application is to provide a porous ceramic, a preparation method thereof, and an atomizer core, and to solve the problem of poor strength of porous ceramics in the prior art.

[0005] In order to solve the above technical problems, an embodiment of the present application provides a porous ceramic, which includes the following raw materials: a skeleton material, boron oxide, illite, a glass material and a pore-forming agent.

[0006] Furthermore, in terms of mass percentage, the skeleton material is 40%-50%, the boron oxide is 3%-5%, the illite is 6%-14%, the glass material is 8%-15%, and the pore-forming agent is 30%-40%.

[0007] Further, the pore-forming agent is hollow glass microspheres, the diameter of the hollow glass microspheres is 20um-100um, and / or the component of the hollow glass microspheres is silicon dioxide; and / or

[0008] The glass material is low-temperature glass with a melting temperature less than or equal to 500°C.

[0009] Furthermore, the framework material includes at least one of potassium feldspar and sodium feldspar.

[0010] The present application also provides a method for preparing a porous ceramic, comprising the following steps:

[0011] Mechanically ball-milling the skeleton material to obtain skeleton material powder, wherein the skeleton material comprises at least one of potassium feldspar and sodium feldspar;

[0012] Adding boron oxide, illite, glass material and hollow glass microspheres to the skeleton material powder, mixing and mechanically milling to obtain a mixed powder;

[0013] The mixed powder is mixed evenly with a polyvinyl alcohol aqueous solution to obtain a mixture;

[0014] The mixture is pressed into shape by dry pressing to obtain a ceramic green body;

[0015] Drying the ceramic green body to obtain a dried green body;

[0016] The dried green body is placed in a sintering furnace for sintering to obtain the porous ceramic.

[0017] Furthermore, the mesh size of the mixed powder is 300-400 mesh; and / or

[0018] In the mixed powder, by mass percentage, the skeleton material accounts for 40%-50%, the boron oxide accounts for 3%-5%, the illite accounts for 6%-14%, the glass material accounts for 8%-15%, and the hollow glass microspheres account for 30%-40%.

[0019] Furthermore, the mass percentage concentration of the polyvinyl alcohol aqueous solution is 0.9%-1.0%; and / or

[0020] The mass of the polyvinyl alcohol aqueous solution is 5%-7% of the mass of the mixed powder.

[0021] Furthermore, the molding pressure of the dry pressing method is 400MPa-600MPa, and the holding time is 10min-20min; and / or

[0022] In the step of drying the ceramic green body, the drying temperature is 80° C.-100° C., and the drying time is 4 h-6 h.

[0023] Furthermore, in the step of placing the dried green body in a sintering furnace for sintering, the sintering temperature is 500° C.-650° C., and the sintering time is 1 h-2 h; and / or

[0024] The sintering furnace is a programmable temperature-controlled box-type furnace, and the heating rate of the programmable temperature-controlled box-type furnace is 5° C. / min.

[0025] The present application also provides an atomizer core, which is made of porous ceramics. The porous ceramics are the porous ceramics as described above or the porous ceramics prepared by the method as described above.

[0026] Compared with the prior art, the embodiments of the present application have the following beneficial effects:

[0027] The raw materials of the porous ceramic provided by the present invention include skeleton materials, boron oxide, illite, glass materials and pore-forming agents. On the one hand, illite can significantly reduce the sintering temperature under the activation of boron oxide, and at the same time can improve the strength, chemical stability and thermal stability of the porous ceramic; on the other hand, the atomizer core is prepared by using the porous ceramic as described above, which can improve the strength and shock resistance of the atomizer core and reduce the phenomenon that the ceramic matrix of the atomizer core is easily damaged and powdered during assembly. DETAILED DESCRIPTION

[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.

[0030] It should also be understood that the terms used in this specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. As used in the specification of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms "a", "an" and "the" are intended to include plural forms.

[0031] It should be further understood that the term "and / or" used in the present description and the appended claims refers to any and all possible combinations of one or more of the associated listed items, and includes these combinations.

[0032] In order to more fully understand the technical content of the present invention, the technical solution of the present invention is further introduced and illustrated in conjunction with specific embodiments below.

[0033] In order to solve the above technical problems, an embodiment of the present application provides a porous ceramic, which includes the following raw materials: a skeleton material, boron oxide, illite, a glass material and a pore-forming agent.

[0034] In this embodiment, illite has a high aluminum content and potassium content; on the one hand, the high aluminum content will promote the formation of mullite and alumina during the sintering process. Mullite and alumina have excellent mechanical properties such as high strength, high hardness, and high temperature resistance, which can effectively improve the overall strength of porous ceramics; on the other hand, the high potassium content will promote the formation of potassium oxide during the sintering process. The melting point of potassium oxide itself does not exceed 900 degrees. It belongs to a low melting point metal oxide and can reduce the sintering strength of porous ceramics. Boron oxide also has excellent fluxing properties. The combination of illite and boron oxide can produce a synergistic effect and significantly reduce the sintering temperature of ceramics; in addition, during the sintering process, illite and boron oxide can form liquid phases, which can fill the pores between ceramic particles, promote the mass transfer process of liquid phase sintering, help the rearrangement and densification of ceramic particles, and improve the microstructure of ceramics, thereby further improving the strength, chemical stability and thermal stability of porous ceramics.

[0035] In some embodiments, by mass percentage, the skeleton material is 40%-50%, the boron oxide is 3%-5%, the illite is 6%-14%, the glass material is 8%-15%, and the pore-forming agent is 30%-40%. In this embodiment, by reasonably setting the mass ratio of various raw materials, a better sintering effect can be obtained.

[0036] Furthermore, the glass material is low-temperature glass with a melting temperature less than or equal to 500° C. Specifically, low-temperature glass can melt at a relatively low temperature, which helps to significantly reduce the sintering temperature of porous ceramics, inhibit excessive growth of ceramic grains at high temperatures, keep the grains small and uniform, and improve the density and strength of ceramics.

[0037] Furthermore, the pore-forming agent is hollow glass microspheres. In this embodiment, the hollow glass microspheres are used as pore-forming agents, and the hollow glass microspheres melt during the sintering process. After the hollow glass microspheres melt, holes are formed in the ceramic, and a certain amount of holes form a through-hole structure. Using hollow glass microspheres as pore-forming agents to replace traditional organic pore-forming agents can greatly save the degreasing process and degreasing time of the organic pore-forming agent, simplify the preparation process, and improve the work efficiency of the ceramic sintering process.

[0038] Furthermore, the diameter of the hollow glass microspheres is 20um-100um. In this embodiment, the pore size of the porous ceramic can be adjusted by controlling the diameter of the hollow glass microspheres. The diameter of the hollow glass microspheres varies according to different pore size requirements, and this application does not limit this.

[0039] In some optional implementations of this embodiment, the diameter of the hollow glass microspheres is any one of 20um, 30um, 40um, 50um, 60um, 70um, 80um, 90um, 100um, etc., or a range between any two of them.

[0040] In some embodiments, the framework material includes at least one of potassium feldspar and sodium feldspar. In this embodiment, potassium feldspar and sodium feldspar both have a low melting point and can melt at a relatively low temperature and participate in the sintering process, thereby significantly reducing the sintering temperature of the porous ceramic; in addition, potassium feldspar and sodium feldspar, as framework materials, can form a stable structural support during the sintering process, which helps the porous ceramic maintain a high density and strength.

[0041] In some embodiments, a method for preparing a porous ceramic is provided, comprising the following steps:

[0042] Step S11, mechanically ball-milling the framework material to obtain framework material powder, wherein the framework material includes at least one of potassium feldspar and sodium feldspar.

[0043] Step S12: adding boron oxide, illite, glass material and hollow glass microspheres to the skeleton material powder, mixing and mechanically milling to obtain a mixed powder.

[0044] Step S13, uniformly mixing the mixed powder and the polyvinyl alcohol aqueous solution to obtain a mixture.

[0045] Step S14: dry pressing the mixture to obtain a ceramic green body.

[0046] Step S15, drying the ceramic green body to obtain a dried green body.

[0047] Step S16: placing the dried green body in a sintering furnace for sintering to obtain the porous ceramic.

[0048] In this embodiment, illite has a high aluminum content and potassium content; on the one hand, the high aluminum content will promote the formation of mullite and alumina during the sintering process. Mullite and alumina have excellent mechanical properties, such as high strength, high hardness, high temperature resistance, etc., which can effectively improve the overall strength of porous ceramics; on the other hand, the high potassium content will promote the formation of potassium oxide during the sintering process. The melting point of potassium oxide itself does not exceed 900 degrees. It belongs to a low melting point metal oxide and can reduce the sintering strength of porous ceramics. Boron oxide also has excellent fluxing properties. The combination of illite and boron oxide can produce a synergistic effect and significantly reduce the sintering temperature of ceramics; in addition, during the sintering process, illite and boron oxide can form a liquid phase, which can fill the pores between ceramic particles, promote the liquid phase sintering mass transfer process, help the rearrangement and densification of ceramic particles, and improve the microstructure of ceramics, thereby further improving the strength, chemical stability and thermal stability of porous ceramics. In addition, the use of hollow glass microspheres as pore formers instead of traditional organic pore formers does not require degreasing of the pore formers, which can greatly save the degreasing process and degreasing time of the organic pore formers, simplify the preparation process, and improve the work efficiency of the ceramic sintering process.

[0049] In some embodiments, in step S11, the skeleton material powder can be prepared by dry ball milling, the mass ratio of the skeleton material to the zirconium oxide ball is 1:1, and after ball milling for a certain period of time, the powder is sieved through a 300-mesh sieve to obtain the skeleton material powder.

[0050] In some embodiments, in step S12, the mesh size of the obtained mixed powder is 300-400 mesh. In this embodiment, the porosity of the porous ceramic can be adjusted by controlling the mesh size of the mixed powder. The mesh size of the mixed powder is different according to different requirements for the porosity, and this application is not limited here.

[0051] In some optional implementations of this embodiment, the mesh size of the mixed powder is any one of 300 mesh, 320 mesh, 340 mesh, 360 mesh, 380 mesh, 400 mesh, etc., or a range between any two of them.

[0052] In some embodiments, in the mixed powder, by mass percentage, the skeleton material is 40%-50%, the boron oxide is 3%-5%, the illite is 6%-14%, the glass material is 8%-15%, and the hollow glass microspheres are 30%-40%.

[0053] In some embodiments, the mass percentage concentration of the polyvinyl alcohol aqueous solution is 0.9%-1.0%, and the mass of the polyvinyl alcohol aqueous solution is 5%-7% of the mass of the mixed powder. In step S13, polyvinyl alcohol, as an excellent dispersant, can effectively adjust the distribution of the mixed powder and prevent the mixed powder from agglomerating and settling during the preparation process; in addition, through the dispersing effect of polyvinyl alcohol, the fluidity of the mixed powder in the aqueous solution is improved, making the subsequent dry pressing process smoother.

[0054] Furthermore, in step S14, the molding pressure of the dry pressing method is 400MPa-600MPa, and the holding time is 10min-20min.

[0055] Furthermore, in step S15, the drying temperature is 80°C-100°C, and the drying time is 4h-6h.

[0056] Furthermore, in step S16, the sintering furnace is a programmable temperature-controlled box furnace, and the heating rate of the programmable temperature-controlled box furnace is 5°C / min. When the temperature reaches 500°C-650°C, it is kept warm for 1h-2h, and then cooled to room temperature with the furnace to obtain porous ceramics.

[0057] In some embodiments, the prepared porous ceramic has an apparent porosity of 45%-65%, a pore size of 12um-32um, and a flexural strength of 120MPa-220MPa.

[0058] In some embodiments, an atomizer core is provided. The atomizer core is made of the porous ceramic as described above or the porous ceramic prepared by the method as described above, which can improve the strength and shock resistance of the atomizer core and reduce the phenomenon of the ceramic matrix of the atomizer core being easily damaged and powdered during assembly.

[0059] The above scheme is further described below in conjunction with specific implementation examples. The preferred embodiments of the present application are described in detail as follows:

[0060] Embodiment 1:

[0061] The present invention provides a method for preparing a porous ceramic. The preparation method is as follows:

[0062] Step 1, dry-milling potassium feldspar, with the mass ratio of potassium feldspar to zirconium oxide balls being 1:1, and passing through a 300-mesh sieve after ball milling to obtain a skeleton material powder;

[0063] Step 2: Add illite, boron oxide, low-temperature glass powder, and hollow glass microspheres to the above-mentioned skeleton material powder, and mix them thoroughly by low-speed ball milling to obtain a mixed powder. In terms of mass percentage, the skeleton material is 45%, the boron oxide is 4%, the illite is 10%, the glass material is 11%, and the hollow glass microspheres are 30%. The diameter of the hollow glass microspheres is 50 um. After being thoroughly mixed by low-speed ball milling, a mixed powder is obtained, and the mesh number of the mixed powder is 300 mesh.

[0064] Step 3, uniformly mix the mixed powder and the polyvinyl alcohol aqueous solution to obtain a mixture, wherein the mass percentage concentration of the polyvinyl alcohol aqueous solution is 1%, and the mass of the polyvinyl alcohol aqueous solution is 6% of the mass of the mixed powder. ;

[0065] Step 4: Pressing the mixture into a shape by dry pressing to obtain a ceramic green body, wherein the forming pressure of the dry pressing method is 500 MPa and the holding time is 10 min;

[0066] Step 5, drying the ceramic green body to obtain a dried green body, wherein the drying temperature is 90° C. and the drying time is 4 hours;

[0067] Step 6: Place the dried green body in a programmable temperature-controlled box furnace with a heating rate of 5°C / min. When the temperature reaches 580°C, keep it warm for 2 hours, and then cool it to room temperature to obtain porous ceramics.

[0068] Example 2

[0069] The difference from Example 1 is that:

[0070] The diameter of the hollow glass microspheres in step 2 is 20 um.

[0071] Example 3

[0072] The difference from Example 1 is that:

[0073] The diameter of the hollow glass microspheres in step 2 is 100 um.

[0074] Example 4

[0075] The difference from Example 1 is that:

[0076] The mass percentage of the hollow glass microspheres in step 2 is 40%.

[0077] Example 5

[0078] The difference from Example 1 is that:

[0079] The mass percentage of boron oxide in step 2 is 3%.

[0080] Example 6

[0081] The difference from Example 1 is that:

[0082] The mass percentage of boron oxide in step 2 is 5%.

[0083] Example 7

[0084] The difference from Example 1 is that:

[0085] The mass percentage of illite in step 2 is 6%.

[0086] Example 8

[0087] The difference from Example 1 is that:

[0088] The mass percentage of illite in step 2 is 14%.

[0089] Comparative Example 1

[0090] The difference from Example 1 is that:

[0091] The diameter of the hollow glass microspheres in step 2 is 150 um.

[0092] Comparative Example 2

[0093] The difference from Example 1 is that:

[0094] The mass percentage of the hollow glass microspheres in step 2 is 50%.

[0095] Comparative Example 3

[0096] The difference from Example 1 is that:

[0097] The mass percentage of illite in step 2 is 0.

[0098] Comparative Example 4

[0099] The difference from Example 1 is that:

[0100] The mass percentage of boron oxide in step 2 is 0.

[0101] Comparative Example 5

[0102] The difference from Example 1 is that:

[0103] In step 2, the mass percentages of boron oxide and illite are both 0.

[0104] The porous ceramics prepared in Examples 1 to 8 and Comparative Examples 1 to 5 were subjected to performance tests such as porosity, through-hole diameter, and flexural strength, wherein the porosity was measured according to the standard "GB / T 1966-1996 Porous Ceramics Apparent Porosity and Capacity Test Method", the through-hole diameter was measured according to the standard "GB / T 1967-1996 Porous Ceramics Pore Diameter Test Method", and the flexural strength was measured according to the standard "GB / T 1965-1996 Porous Ceramics Flexural Strength Test Method Porous Ceramics Flexural Strength Test Method", and the test results are shown in Table 1 below:

[0105] Table 1

[0106]

[0107]

[0108] It can be seen from the test results in Table 1 that, compared with Comparative Examples 3 to 5, the materials of the mixed powders of Examples 1 to 8 include illite and boron oxide, so that the porous ceramics can significantly improve the flexural strength of the porous ceramics while maintaining a certain porosity. The reason may be that the illite of Examples 1 to 8 has a higher aluminum content and potassium content. The higher aluminum content will promote the formation of mullite and alumina during the sintering process. Mullite and alumina have excellent mechanical properties, such as high strength, high hardness, high temperature resistance, etc., which can effectively improve the overall strength of the porous ceramics; and the higher potassium content will promote the formation of potassium oxide during the sintering process. Potassium chloride is a low-melting-point metal oxide that can reduce the sintering strength of porous ceramics; and boric oxide also has excellent fluxing properties. The combination of illite and boric oxide can produce a synergistic effect, significantly reducing the sintering temperature of ceramics and reducing the pores in the ceramics that are gradually sintered away due to excessive temperature, thereby ensuring that the ceramics can maintain a certain porosity; in addition, during the sintering process, illite and boric oxide can form a liquid phase, which can fill the pores between ceramic particles, promote the liquid phase sintering mass transfer process, help the rearrangement and densification of ceramic particles, and improve the microstructure of the ceramic, thereby further improving the strength of porous ceramics.

[0109] According to the test results of porous ceramic embodiments 1 to 4 and porous ceramic comparison examples 1 and 2, it can be learned that by appropriately setting the diameter and mass fraction of the hollow glass microspheres, it can be further ensured that the porosity and pore size of the porous ceramics meet the use requirements, and can achieve a certain bending strength, meeting the product requirements.

[0110] References throughout the specification to "some embodiments", "partial embodiments", "one embodiment", "another example", "example", "specific example" or "partial example" mean that at least one embodiment or example in the present application includes the specific features, structures, materials or characteristics described in the embodiment or example. Therefore, descriptions appearing in various places throughout the specification, such as: "in some embodiments", "in an embodiment", "in one embodiment", "in another example", "in an example", "in a specific example" or "example", do not necessarily refer to the same embodiment or example in the present application. In addition, the specific features, structures, materials or characteristics herein may be combined in one or more embodiments or examples in any suitable manner.

[0111] Although illustrative embodiments have been demonstrated and described, those skilled in the art should understand that the above embodiments should not be construed as limitations on the present application, and that changes, substitutions and modifications may be made to the embodiments without departing from the spirit, principles and scope of the present application.

Claims

1. A porous ceramic, characterized in that: The raw materials include: framework material, boron oxide, illite, glass material and pore-forming agent.

2. The porous ceramic according to claim 1, characterized in that: In terms of mass percentage, the skeleton material accounts for 40%-50%, the boron oxide accounts for 3%-5%, the illite accounts for 6%-14%, the glass material accounts for 8%-15%, and the pore-forming agent accounts for 30%-40%.

3. The porous ceramic according to claim 1, characterized in that: The pore-forming agent is hollow glass microspheres, the diameter of the hollow glass microspheres is 20um-100um, and / or the component of the hollow glass microspheres is silicon dioxide; and / or The glass material is low-temperature glass with a melting temperature less than or equal to 500°C.

4. The porous ceramic according to claim 1, characterized in that: The framework material includes at least one of potassium feldspar and sodium feldspar.

5. A method for preparing porous ceramics, characterized in that: The steps include: Mechanically ball-milling the skeleton material to obtain skeleton material powder, wherein the skeleton material comprises at least one of potassium feldspar and sodium feldspar; Adding boron oxide, illite, glass material and hollow glass microspheres to the skeleton material powder, mixing and mechanically milling to obtain a mixed powder; The mixed powder is mixed evenly with a polyvinyl alcohol aqueous solution to obtain a mixture; The mixture is pressed into shape by dry pressing to obtain a ceramic green body; Drying the ceramic green body to obtain a dried green body; The dried green body is placed in a sintering furnace for sintering to obtain the porous ceramic.

6. The preparation method according to claim 5, characterized in that: The mesh size of the mixed powder is 300-400 mesh; and / or In the mixed powder, by mass percentage, the skeleton material accounts for 40%-50%, the boron oxide accounts for 3%-5%, the illite accounts for 6%-14%, the glass material accounts for 8%-15%, and the hollow glass microspheres account for 30%-40%.

7. The preparation method according to claim 5, characterized in that: The mass percentage concentration of the polyvinyl alcohol aqueous solution is 0.9%-1.0%; and / or The mass of the polyvinyl alcohol aqueous solution is 5%-7% of the mass of the mixed powder.

8. The preparation method according to claim 5, characterized in that: The molding pressure of the dry pressing method is 400MPa-600MPa, and the holding time is 10min-20min; and / or In the step of drying the ceramic green body, the drying temperature is 80° C.-100° C., and the drying time is 4 h-6 h.

9. The preparation method according to claim 5, characterized in that: In the step of placing the dried green body in a sintering furnace for sintering, the sintering temperature is 500° C.-650° C., and the sintering time is 1 h-2 h; and / or The sintering furnace is a programmable temperature-controlled box-type furnace, and the heating rate of the programmable temperature-controlled box-type furnace is 5° C. / min.

10. An atomizer core, characterized in that: The atomizing core is made of porous ceramics, and the porous ceramics are the porous ceramics described in any one of claims 1-4 or the porous ceramics prepared by the method described in any one of claims 5-9.

Citation Information

Cited By

  • High-porosity and high-strength thin-wall cordierite honeycomb ceramic and preparation method thereof