Reversible photochromic compound as well as preparation method and application thereof
Synthesizing reversible photochromic compounds through organic coupling reactions and combining solid matrix coating technology, the problem of slow response speed and unstable discoloration performance of photochromic materials is solved, and the material's response speed is improved and the discoloration stability is excellent. In delay encryption anti-counterfeiting strategy.
Patent Information
- Application Number
- CN202410990168.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The existing photochromic materials have slow response speed, unstable discoloration performance, short life, high preparation cost and aggregation-induced quenching problems, which limit their performance and popularity in practical applications.
The reversible photochromic compounds were synthesized by organic coupling reaction, and the condensation and reflux reaction was carried out in tetrahydrofuran/water solution by benzothiophene derivative and potassium carbonate in tetrahydrofuran/water solution was prepared in combination with solid matrix coating method to achieve ultraviolet light and visible light The color change of alternating responses is improved by aggregation-induced luminescence characteristics.
It has achieved improved response speed of the material, excellent color change stability, extended service life, and reduced preparation cost. The material has non-contact light response anti-counterfeiting capabilities, which is suitable for delay encryption and anti-counterfeiting strategies.
Smart Images

Figure CN118930515A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of reversible photochromic materials. Background Art
[0002] In the context of the rapidly developing digital age, information is interacted through various channels, and the risk of information leakage has also increased exponentially. Information protection has become a current research hotspot, and more advanced and secure anti-counterfeiting technologies are considered necessary to encrypt and protect important information such as banknotes, identity passports, and confidential documents. Therefore, researchers have created a series of anti-counterfeiting materials with various stimulus response characteristics. Among them, light-responsive functional materials have the advantages of simple processing, high yield, and precise design, which can realize encrypted storage and secure reading of information.
[0003] Cellulose is a natural polymer that is widely present in plant cell walls and is one of the most abundant organic substances on earth. It exists in the form of microfibrils in plant cell walls, providing structural support for plants. Due to its renewability and independence from fossil fuels, the use of biological resources to produce valuable materials for industrial use has attracted a lot of attention in recent years. As one of the cheapest and most widely used raw materials on earth, cellulose can be used to synthesize environmentally friendly, green and sustainable functional materials. In addition, as a colorless and odorless biopolymer, cellulose has unique advantages, including high biocompatibility, renewable sustainability, easy degradation, easy chemical modification of polyhydroxyl structure, heat resistance, and strong adsorption capacity. Among them, cellulose can be modified into various useful materials, and chemical modification in smart fluorescent materials gives cellulose more application possibilities. Further, due to the excellent plasticity of cellulose, the prepared fluorescent cellulose materials are made into films, fibers, paper tapes, carbon dots, hydrogels and solutions. These materials have fluorescent responses to toxic metals and anions, pH values, and common organic solvents or can be used for fluorescent printing and coating. These characteristics give cellulose a huge advantage in the field of anti-counterfeiting applications.
[0004] Photochromic materials are materials that can change color by light exposure. They have broad application prospects in smart glasses, smart windows, photosensitizing dyes and other fields. However, there are still a series of technical defects in current photochromic materials, which not only limit their performance in practical applications, but also hinder their further development and application. First, the current photochromic materials are insufficient in response speed. The color change speed of some materials is slow and cannot meet the needs of real-time changes, such as the response speed required to quickly adjust the color of smart glasses lenses. In addition, some materials may have color stability problems after long-term use, resulting in uneven or distorted color changes, affecting user experience and material reliability. Secondly, the durability of photochromic materials is also a problem worthy of attention. Long-term light exposure or frequent color change operations may cause material performance degradation or failure, thereby reducing the service life and reliability of the material and increasing maintenance and replacement costs. In addition, the cost of photochromic materials is relatively high, mainly due to the cost of the material itself and the complexity of preparation and processing, which limits the popularization and promotion of photochromic technology in large-scale applications, especially for consumer products that require high cost-effectiveness. In addition, most photochromic switches often suffer from aggregation quenching caused by aggregation, which limits their application in various fields. These problems together affect the further development and application of photochromic technology. Therefore, solving these technical defects and improving the performance and reliability of photochromic materials is one of the important directions for the development of current photochromic technology. Summary of the invention
[0005] The present invention aims to solve the problems of slow response speed, unstable color change performance, short life, high preparation cost, complex synthesis and aggregation-induced quenching in existing photochromic materials, and further provide a reversible photochromic compound and its preparation method and application.
[0006] Reversible photochromic compound, the structural formula of the reversible photochromic compound is
[0007] The preparation method of the reversible photochromic compound is carried out according to the following steps:
[0008] The intermediate, the benzothiophene derivative and potassium carbonate are dissolved in a mixed solution of tetrahydrofuran / water, and then tetrakis(triphenylphosphine)palladium is added under nitrogen protection, and the reaction is carried out under condensation reflux for 17h to 48h under a nitrogen atmosphere and a temperature of 60° C. to 90° C. After the reaction is completed, the volatile solvent is removed by reduced pressure distillation, and then the organic phase is extracted three times with ethyl acetate and deionized water, and the organic phase is dried with anhydrous magnesium sulfate. Finally, a mixed solution of dichloromethane / petroleum ether is used as an eluent for column chromatography purification to obtain a reversible photochromic compound;
[0009] The structural formula of the intermediate is The benzothiophene derivative is benzothiophene-3-boric acid or 3-bromobenzothiophene.
[0010] The invention discloses an application of a reversible photochromic compound, and it is used for the preparation of a reversible photochromic material.
[0011] The beneficial effects of the present invention are:
[0012] 1. The present invention utilizes organic coupling reaction, the material synthesis route is simple, and the preparation cost is low; based on the reversible photochromic property and combined with the concept of aggregation-induced emission, a new compound with aggregation-induced emission properties and capable of alternately responding to ultraviolet light and visible light is constructed, and single crystals are successfully cultivated;
[0013] 2. The present invention is based on the reversible change characteristics of the color-changing filter paper material in response to light, which can realize the reversible disappearance and recovery of information after reading, improve fatigue resistance and can be reused when combined with paper, which is green and environmentally friendly.
[0014] 3. The present invention solves the problem of photochromic material photooxidation by using a solid matrix coating method, and prepares photochromic PMMA film, cellulose film and cellulose composite film. After a series of optical characterizations, it is proved that the composite film is superior to the first two films and has a long service life.
[0015] Fourth, the present invention realizes a non-contact light-responsive anti-counterfeiting method based on the photochromic characteristics of different irradiated light, and the synthesis of photochromic molecules is simple, and the color change stability of the material is excellent, which makes it have the advantages of fast response, no pollution of coded information, and excellent reversibility compared with contact chemical anti-counterfeiting methods;
[0016] 5. The present invention is based on three materials to make different photochromic films. Through the difference in recovery time of the response to visible light after color change, time-delayed information protection can be added to the traditional anti-counterfeiting field level to achieve a delayed encryption anti-counterfeiting strategy.
[0017] Instruction Manual
[0018] Figure 1 The hydrogen nuclear magnetic resonance spectrum of the 2PBS compound prepared in Example 1;
[0019] Figure 2 The high-resolution mass spectrum of the 2PBS compound prepared in Example 1;
[0020] Figure 3 The H NMR spectrum of the HPBS compound prepared in Example 2;
[0021] Figure 4The high resolution mass spectrum of the HPBS compound prepared in Example 2;
[0022] Figure 5 The hydrogen nuclear magnetic resonance spectrum of the 2PSF compound prepared in Example 3;
[0023] Figure 6 This is a high-resolution mass spectrum of the 2PSF compound prepared in Example 3;
[0024] Figure 7 Schematic diagram of the photochemical phenomena of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 in different states;
[0025] Figure 8 Schematic diagram of the molecular structure changes of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 under ultraviolet light (365 nm);
[0026] Fig. 9 The fluorescence spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 changing with time under continuous ultraviolet light irradiation in tetrahydrofuran;
[0027] Fig.10 The UV-visible absorption spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 changing with time under continuous UV irradiation in tetrahydrofuran;
[0028] Fig.11 The time-resolved fluorescence decay curves of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3;
[0029] Fig.12 The fluorescence spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 at different water contents in tetrahydrofuran / water solution and the fluorescence intensity dot-line graph;
[0030] Fig.13 Photochromic cycle test diagram of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3, which were alternately exposed to ultraviolet light (365 nm) and visible light in a tetrahydrofuran solution;
[0031] Fig.14 This is a photo-controlled patterning application diagram of the reversible photochromic filter paper prepared in Example 4; in the figure, the initial filter paper does not show a pattern;
[0032] Fig.15The photochromic cycle test diagram of the 2PSF@PMMA film prepared in Example 5 and the 2PSF@HPC film prepared in Example 6 when alternately exposed to ultraviolet light and visible light;
[0033] Fig.16 The UV-visible absorption spectra of the 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 that change with time under continuous UV irradiation;
[0034] Fig.17 Photochromic cycle test diagram of 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7, alternately exposed to ultraviolet light (365 nm) and visible light;
[0035] Fig.18 The relationship curve between the normalized absorbance value and the recovery time of the 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7;
[0036] Fig.19 The QR code labels based on the photochromic films with different isomerization rates prepared in Example 7;
[0037] Fig. 20 Single crystal structure diagram of 2PBS, HPBS, and 2PSF. DETAILED DESCRIPTION
[0038] Specific implementation method 1: This implementation method is a reversible photochromic compound, and the structural formula of the reversible photochromic compound is
[0039] This specific embodiment achieves the color change of a single molecule under the alternating action of ultraviolet light and visible light by preparing photochromic compounds with aggregation-induced luminescence. Afterwards, various compounds are combined with filter paper, polymethyl methacrylate, and hydroxypropyl cellulose to prepare single-layer films and composite films, enhance the antioxidant properties of the molecules, achieve multi-color reversible photochromism of cellulose, and conduct anti-counterfeiting strategy research.
[0040] This specific embodiment combines traditional photochromic molecules with the concept of aggregation-induced emission (AIE) to achieve color changes under the alternating action of ultraviolet light and visible light, as well as photochromic molecules with AIE effect. The design and synthesis are simple, the material stability is good, and the application is wide, providing a new strategy for light-controlled information encryption and protection. It involves applications such as photolithography patterns, optical anti-counterfeiting, and the preparation of multi-color cellulose composite films to improve their fatigue resistance.
[0041] The beneficial effects of this embodiment are:
[0042] 1. This embodiment uses an organic coupling reaction, the material synthesis route is simple, and the preparation cost is low; based on the reversible photochromic properties and combined with the concept of aggregation-induced emission, a new compound with aggregation-induced emission properties and capable of alternately responding to ultraviolet light and visible light is constructed, and single crystals are successfully cultivated;
[0043] 2. This embodiment is based on the reversible change characteristics of the color-changing filter paper material in response to light, which can achieve reversible disappearance and recovery of information after reading, improve fatigue resistance and can be reused when combined with paper, which is green and environmentally friendly.
[0044] 3. This embodiment cleverly solves the problem of photochromic material photooxidation by using a solid matrix coating method, and prepares photochromic PMMA film, cellulose film and cellulose composite film. After a series of optical characterizations, it is proved that the composite film is superior to the first two films and has a long service life.
[0045] Fourth, this embodiment realizes a non-contact light-responsive anti-counterfeiting method based on the photochromic characteristics of different irradiated light, and the photochromic molecule synthesis is simple, and the color change stability of the material is excellent, which makes it have the advantages of fast response, no pollution of encoded information, and excellent reversibility compared with contact chemical anti-counterfeiting methods;
[0046] 5. This embodiment uses three materials to make different photochromic films. Through the difference in recovery time of the response to visible light after color change, it can increase time-delay information protection at the level of traditional anti-counterfeiting field and realize the anti-counterfeiting strategy of delayed encryption.
[0047] Specific embodiment 2: The preparation method of the reversible photochromic compound in this embodiment is carried out according to the following steps:
[0048] The intermediate, the benzothiophene derivative and potassium carbonate are dissolved in a mixed solution of tetrahydrofuran / water, and then tetrakis(triphenylphosphine)palladium is added under nitrogen protection, and the reaction is carried out under condensation reflux for 17h to 48h under a nitrogen atmosphere and a temperature of 60° C. to 90° C. After the reaction is completed, the volatile solvent is removed by reduced pressure distillation, and then the organic phase is extracted three times with ethyl acetate and deionized water, and the organic phase is dried with anhydrous magnesium sulfate. Finally, a mixed solution of dichloromethane / petroleum ether is used as an eluent for column chromatography purification to obtain a reversible photochromic compound;
[0049] The structural formula of the intermediate is The benzothiophene derivative is benzothiophene-3-boric acid or 3-bromobenzothiophene.
[0050] Specific embodiment 3: This embodiment differs from specific embodiment 2 in that: the molar ratio of the intermediate to the benzothiophene derivative is 1:(2-2.6); the molar ratio of the intermediate to potassium carbonate is 1:(2.5-3.5); the molar ratio of the intermediate to tetrakis(triphenylphosphine)palladium is 1:(0.05-0.1); the volume ratio of the molar amount of the intermediate to the mixed solution of tetrahydrofuran / water is 1mmol:(25-35)mL; the volume ratio of tetrahydrofuran to water in the mixed solution of tetrahydrofuran / water is 1:(0.35-0.45); the volume ratio of dichloromethane to petroleum ether in the mixed solution of dichloromethane / petroleum ether is 1:(4-12). Others are the same as specific embodiment 2.
[0051] Specific implementation method 4: The application of the reversible photochromic compound in this implementation method is used for the preparation of reversible photochromic materials.
[0052] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the reversible photochromic material changes color under the alternating action of ultraviolet light and visible light. The rest is the same as specific embodiment 4.
[0053] Specific embodiment 6: This embodiment is different from specific embodiment 4 or 5 in that the reversible photochromic material is a reversible photochromic filter paper, a reversible photochromic polymethyl methacrylate film, a reversible photochromic hydroxypropyl cellulose film or a reversible photochromic cellulose composite film. The rest is the same as specific embodiment 4 or 5.
[0054] Specific embodiment 7: This embodiment is different from any one of specific embodiments 4 to 6 in that: when the reversible photochromic material is a reversible photochromic filter paper, it is specifically prepared according to the following steps:
[0055] The reversible photochromic compound is dissolved in dichloromethane to obtain a transparent solution, the filter paper is immersed in the transparent solution at room temperature for 6 hours to 12 hours, and then dried to obtain the reversible photochromic filter paper; the mass ratio of the filter paper size to the reversible photochromic compound in the transparent solution is 1 cm 2 : (0.5-1) mg; the concentration of the reversible photochromic compound in the transparent solution is 1 mol / L-2 mol / L. The rest is the same as the specific embodiments 4 to 6.
[0056] Specific embodiment eight: This embodiment differs from any one of specific embodiments four to seven in that when the reversible photochromic material is a reversible photochromic polymethyl methacrylate film, it is prepared according to the following steps:
[0057] Dissolve polymethyl methacrylate and a reversible photochromic compound in dichloromethane to obtain a transparent solution; pour the transparent solution into a mold and evaporate and dry naturally at room temperature to obtain a reversible photochromic polymethyl methacrylate film; the mass ratio of the polymethyl methacrylate to the reversible photochromic compound is 1:(0.05-0.2); the mass ratio of the polymethyl methacrylate to dichloromethane is 1 mg:(0.5-1) mL. Others are the same as Specific Embodiments 4 to 7.
[0058] Specific embodiment 9: This embodiment is different from any one of specific embodiments 4 to 8 in that when the reversible photochromic material is a reversible photochromic hydroxypropyl cellulose film, it is prepared according to the following steps:
[0059] The reversible photochromic compound is dissolved in dimethyl sulfoxide to obtain a transparent solution; hydroxypropyl cellulose is added to distilled water to obtain a hydroxypropyl cellulose aqueous solution; the transparent solution is mixed with the hydroxypropyl cellulose aqueous solution to obtain a mixed solution; the mixed solution is poured into a mold, heated and dried at a temperature of 60°C to 65°C to obtain a reversible photochromic hydroxypropyl cellulose film; the mass ratio of the reversible photochromic compound to the volume of dimethyl sulfoxide is 1 mg: (0.05 to 0.2) mL; the mass ratio of the hydroxypropyl cellulose to the volume of distilled water is 1 mg: (0.5 to 1) mL; the mass ratio of the hydroxypropyl cellulose to the reversible photochromic compound in the mixed solution is 1: (0.05 to 0.25). The rest is the same as the specific embodiments four to eight.
[0060] Specific embodiment 10: This embodiment is different from any one of specific embodiments 4 to 9 in that: when the reversible photochromic material is a reversible photochromic cellulose composite film, it is specifically prepared according to the following steps:
[0061] The reversible photochromic compound is dissolved in dimethyl sulfoxide to obtain a transparent solution; hydroxypropyl cellulose is added to distilled water to obtain a hydroxypropyl cellulose aqueous solution; the transparent solution is mixed with the hydroxypropyl cellulose aqueous solution to obtain a mixed solution; the mixed solution is poured into a mold covered with a PMMA film, heated and dried at a temperature of 60°C to 65°C, and then the PMMA solution is poured onto the surface, and heated and dried again at a temperature of 60°C to 65°C to form a PMMA / cellulose / PMMA structure, thereby obtaining a reversible photochromic cellulose composite film; The mass ratio of the reversible photochromic compound to the volume ratio of dimethyl sulfoxide is 1 mg: (0.05-0.2) mL; the mass ratio of the hydroxypropyl cellulose to the volume ratio of distilled water is 1 mg: (0.5-1) mL; the mass ratio of the hydroxypropyl cellulose to the reversible photochromic compound in the mixed solution is 1: (0.05-0.25); the thickness of the single-sided PMMA film is 0.1 mm-0.5 mm; the mass ratio of the single-sided PMMA to the reversible photochromic compound in the reversible photochromic cellulose composite film is 1: (0.1-0.2). Others are the same as the fourth to ninth embodiments.
[0062] The following examples are used to verify the beneficial effects of the present invention:
[0063] Embodiment 1:
[0064] The preparation method of the reversible photochromic compound is carried out according to the following steps:
[0065] 1. Preparation of intermediates:
[0066] Under the conditions of nitrogen atmosphere and rotation speed of 1000 rpm, benzophenone (0.912 g, 5 mmol), carbon tetrabromide (3.318 g, 10 mmol) and triphenylphosphine (5.259 g, 20 mmol) were added to 50 mL of anhydrous toluene, and then the reaction system was heated to 140 ° C., and stirred for 4 days under the conditions of nitrogen atmosphere, rotation speed of 600 rpm and temperature of 140 ° C. After the reaction was completed, it was cooled to room temperature, and the filtrate was filtered and dried to obtain a black oily substance; petroleum ether was used as an eluent for column chromatography purification to obtain a yellow liquid, which was an intermediate, with a yield of 40%;
[0067] The structural formula of the intermediate is It is named as 2PBS intermediate;
[0068] 2. The intermediate (1.05 g, 0.6 mmol), benzothiophene-3-boric acid (1.3 g, 1.44 mmol) and potassium carbonate (1.25 g, 1.8 mmol) were dissolved in a mixed solution of 20 mL of tetrahydrofuran / water (V / V=7:3), and then tetrakis(triphenylphosphine)palladium (200 mg, 0.03 mmol) was added under nitrogen protection, and the mixture was condensed and refluxed under a nitrogen atmosphere at a temperature of 85°C for 48 h. After the reaction was completed, the volatile solvent was removed by reduced pressure distillation, and then the mixture was extracted three times with ethyl acetate and deionized water. The organic phase was dried with anhydrous magnesium sulfate, and finally a mixed solution of dichloromethane / petroleum ether was used as an eluent for column chromatography purification to obtain a reversible photochromic compound with a yield of 35%;
[0069] The structural formula of the reversible photochromic compound is It was named as 2PBS compound;
[0070] The volume ratio of dichloromethane to petroleum ether in the dichloromethane / petroleum ether mixture is 1:5.
[0071] The reaction equation of step one is as follows:
[0072]
[0073] The reaction equation of step 2 is as follows:
[0074]
[0075] Embodiment 2:
[0076] The preparation method of the reversible photochromic compound is carried out according to the following steps:
[0077] 1. Preparation of intermediates:
[0078] Under the conditions of nitrogen atmosphere and rotation speed of 800rpm, carbon tetrabromide (3.318g, 10mmol) and triphenylphosphine (5.259g, 20mmol) were respectively added dropwise to 30mL of anhydrous dichloromethane to obtain carbon tetrabromide solution and triphenylphosphine solution; under the conditions of nitrogen atmosphere and rotation speed of 600rpm, the carbon tetrabromide solution was added dropwise to the triphenylphosphine solution, stirred for 10min, then benzaldehyde (0.531g, 5mmol) was added, the system was protected by nitrogen and sealed, stirred at room temperature for 2h, filtered and the filtrate was spin-dried to obtain a black oily substance; then petroleum ether was used as an eluent for column chromatography purification to obtain a transparent liquid, i.e., an intermediate, with a yield of 76%;
[0079] The structural formula of the intermediate is It is named as HPBS intermediate;
[0080] 2. The intermediate (1.05 g, 1 mmol), benzothiophene-3-boric acid (1.7 g, 2.4 mmol) and potassium carbonate (1.66 g, 3 mmol) were dissolved in a 30 mL tetrahydrofuran / water (V / V=7:3) mixed solution, and then tetrakis(triphenylphosphine)palladium (232 mg, 0.05 mmol) was added under nitrogen protection, and the mixture was condensed and refluxed under a nitrogen atmosphere at a temperature of 85°C for 48 h. After the reaction was completed, the volatile solvent was removed by reduced pressure distillation, and then the mixture was extracted three times with ethyl acetate and deionized water. The organic phase was dried with anhydrous magnesium sulfate, and finally a mixed solution of dichloromethane / petroleum ether was used as an eluent for column chromatography purification to obtain a reversible photochromic compound with a yield of 56%.
[0081] The structural formula of the reversible photochromic compound is It was named as HPBS compound;
[0082] The volume ratio of dichloromethane to petroleum ether in the dichloromethane / petroleum ether mixture is 1:12.
[0083] The reaction equation of step one is as follows:
[0084]
[0085] The reaction equation of step 2 is as follows:
[0086]
[0087] Embodiment 3:
[0088] The preparation method of the reversible photochromic compound is carried out according to the following steps:
[0089] 1. Preparation of intermediates:
[0090] Diboric acid pinacol ester (4 g, 4 mmol) and tetrakis(triphenylphosphine) platinum (90 mg, 0.1 mmol) were placed in a reaction bottle, and diphenylacetylene (1.24 g, 7 mmol) and 50 mL of N,N-dimethylformamide were added under a nitrogen atmosphere, and then the reaction was carried out at a temperature of 90° C. for 24 h. After the reaction was completed, the mixture was cooled to room temperature, extracted three times with ethyl acetate and deionized water, and the organic phase was dried with anhydrous magnesium sulfate, and the crude product was obtained by rotary drying under reduced pressure. Finally, the white solid was washed with anhydrous ethanol for several times, which was the intermediate, and the yield was 42%;
[0091] The structural formula of the intermediate is It is named as 2PSF intermediate;
[0092] 2. The intermediate (1.3 g, 3 mmol), 3-bromobenzothiophene (1.5 g, 7.2 mmol) and potassium carbonate (1.3 g, 9 mmol) were dissolved in 90 mL of a mixed solution of tetrahydrofuran / water (V / V=7:3), and then tetrakis(triphenylphosphine)palladium (170 mg, 0.15 mmol) was added under nitrogen protection, and the mixture was condensed and refluxed under a nitrogen atmosphere at 85°C for 48 h. After the reaction was completed, the volatile solvent was removed by reduced pressure distillation, and then the mixture was extracted three times with ethyl acetate and deionized water. The organic phase was dried with anhydrous magnesium sulfate, and finally a mixed solution of dichloromethane / petroleum ether was used as an eluent for column chromatography purification to obtain a reversible photochromic compound with a yield of 65%.
[0093] The structural formula of the reversible photochromic compound is It is named as 2PSF compound;
[0094] The volume ratio of dichloromethane to petroleum ether in the dichloromethane / petroleum ether mixture is 1:4.
[0095] The reaction equation of step one is as follows:
[0096]
[0097] The reaction equation of step 2 is as follows:
[0098]
[0099] Embodiment 4:
[0100] The reversible photochromic compound (2PSF compound) prepared in Example 3 was used to prepare the reversible photochromic filter paper, specifically according to the following steps:
[0101] 8 mg (0.018 mol) of the reversible photochromic compound (2PSF compound) prepared in Example 3 was dissolved in 15 mL of dichloromethane to obtain a transparent solution. A 4 cm×4 cm filter paper was immersed in the transparent solution at room temperature for 8 h and then dried to obtain a reversible photochromic filter paper.
[0102] Embodiment 5:
[0103] The reversible photochromic polymethyl methacrylate film was prepared by using the reversible photochromic compounds (2PBS compound, HPBS compound, 2PSF compound) prepared in Examples 1 to 3, respectively, specifically according to the following steps:
[0104] 15 mg of polymethyl methacrylate and 1.8 mg of a reversible photochromic compound were dissolved in 10 mL of dichloromethane to obtain a transparent solution. The transparent solution was poured into a mold and naturally evaporated and dried at room temperature to obtain a reversible photochromic polymethyl methacrylate film, which was named 2PBS@PMMA film, HPBS@PMMA film, and 2PSF@PMMA film, respectively.
[0105] Embodiment 6:
[0106] The reversible photochromic compounds (2PBS compound, HPBS compound, 2PSF compound) prepared in Examples 1 to 3 were used to prepare reversible photochromic hydroxypropyl cellulose films, specifically according to the following steps:
[0107] 10 mg of reversible photochromic compound was dissolved in 2 mL of dimethyl sulfoxide to obtain a transparent solution; 50 mg of hydroxypropyl cellulose was added to 25 mL of distilled water to obtain a hydroxypropyl cellulose aqueous solution; 1 mL of the transparent solution was mixed with 10 mL of the hydroxypropyl cellulose aqueous solution to obtain a mixed solution; the mixed solution was poured into a mold, heated and dried at 60°C to obtain reversible photochromic hydroxypropyl cellulose films, which were named 2PBS@HPC, HPBS@HPC, and 2PSF@HPC films, respectively.
[0108] Embodiment 7:
[0109] The reversible photochromic cellulose composite films were prepared by using the reversible photochromic compounds (2PBS compound, HPBS compound, 2PSF compound) prepared in Examples 1 to 3, respectively, and were prepared according to the following steps:
[0110] 10 mg of a reversible photochromic compound was dissolved in 2 mL of dimethyl sulfoxide to obtain a transparent solution; 50 mg of hydroxypropyl cellulose was added to 25 mL of distilled water to obtain a hydroxypropyl cellulose aqueous solution; 1 mL of the transparent solution was mixed with 10 mL of the hydroxypropyl cellulose aqueous solution to obtain a mixed solution; the mixed solution was poured into a mold covered with a PMMA film, heated and dried at 60° C., and then a PMMA solution was poured onto the surface, and heated and dried again at 60° C. to form a PMMA / cellulose / PMMA structure, thereby obtaining a reversible photochromic cellulose composite film, which was named 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA, respectively; the thickness of the single-sided PMMA film was 0.3 mm; and the mass ratio of the single-sided PMMA to the reversible photochromic compound in the reversible photochromic cellulose composite film was 1:0.1.
[0111] Figure 1The hydrogen nuclear magnetic resonance spectrum of the 2PBS compound prepared in Example 1; the hydrogen nuclear magnetic resonance spectrum uses deuterated chloroform as a deuterated reagent, and after integration processing, it is shown that the single peak appearing at 7.12ppm is attributed to the hydrogen on thiophene, and the double peak appearing at 7.44ppm and 7.75ppm is attributed to the hydrogen on both sides of benzothiophene. The triplet appearing at 7.12ppm is the attributed hydrogen of the benzene ring of benzothiophene. The split peaks appearing at 7.10ppm and 7.06ppm are attributed to the attributed hydrogen on the benzene ring connected to the double bond. And the total number of hydrogen after integration is 20, corresponding to the number of molecular hydrogen, indicating that the 2PBS product is successfully synthesized.
[0112] Figure 2 This is the high-resolution mass spectrum of the 2PBS compound prepared in Example 1; as can be seen from the figure, the peak data in the high-resolution mass spectrum is the test data, and the molecular weight result is 444.762, which is consistent with the actual molecular weight M=444, proving that the 2PBS product was successfully synthesized.
[0113] Figure 3 The HPBS compound prepared in Example 2 is shown in the HMR spectrum; the HMR spectrum uses deuterated chloroform as a deuterated reagent, and after integration, the triplet peak at 8.02ppm, the doublet peak at 7.96ppm and 7.64ppm are attributed to the hydrogen of the benzene ring on both sides of the benzothiophene, and the triplet peak at 7.30ppm is attributed to the hydrogen on the benzene ring on the left side of the double bond. The split peaks at 7.45ppm and 7.43ppm are hydrogens in the aromatic region. And the total number of hydrogens after integration is 16, corresponding to the number of molecular hydrogens, indicating that the HPBS product is successfully synthesized.
[0114] Figure 4 This is the high-resolution mass spectrum of the HPBS compound prepared in Example 2; as can be seen from the figure, the peak data in the high-resolution mass spectrum is the test data, and the molecular weight result is 369.02, which is consistent with the actual molecular weight M=368, proving that the HPBS product was successfully synthesized.
[0115] Figure 5 This is the hydrogen nuclear magnetic resonance spectrum of the 2PSF compound prepared in Example 3; the hydrogen nuclear magnetic resonance spectrum uses deuterated chloroform as the deuterated reagent, and after integration processing, it is shown that the single peak appearing at 7.01ppm is attributed to the hydrogen on the thiophene, and the double peaks appearing at 7.69ppm and 7.31ppm are attributed to the hydrogen on the benzene rings of benzothiophene on both sides. The triplet appearing at 7.06ppm is the attributed hydrogen of the benzene ring on the same side of the double bond. The split peaks appearing at 7.17ppm and 7.14ppm are attributed to the attributed hydrogen in the aromatic region. And the total number of hydrogen after integration is 20, which corresponds to the number of molecular hydrogen, indicating that the 2PSF product has been successfully synthesized.
[0116] Figure 6This is the high-resolution mass spectrum of the 2PSF compound prepared in Example 3; as can be seen from the figure, the peak data in the high-resolution mass spectrum is the test data, and the molecular weight result is 444.776, which is consistent with the actual molecular weight M=444, proving that the 2PSF product was successfully synthesized.
[0117] The compounds prepared in Examples 1 to 3 are arylethylene compounds containing benzothiophene; Figure 7 Schematic diagram of the photochemical phenomena of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 in different states; as can be seen from the figure, the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 have differences in different states, have obvious photophysical changes, that is, changes in color visible to the naked eye, and in the solid powder state, different and obvious color changes occur after ultraviolet light excitation (power of 10 W, wavelength of 365 nm), and can be irradiated with visible light (power of 1.5 W, wavelength of 524 nm). The color of 2PBS, HPBS and 2PSF can be restored to the initial state after being irradiated with visible light for 30 seconds. For example, 2PBS is a light yellow solid powder, which changes to orange after being irradiated with ultraviolet light for 10 seconds. HPBS is a beige solid powder, which changes to orange after being irradiated with ultraviolet light for 10 seconds. 2PSF is a white solid powder, which changes to purple after being irradiated with ultraviolet light for 10 seconds. Moreover, 2PBS, HPBS and 2PSF solid powders can be restored to their initial colors after being irradiated with visible light for 30 seconds. Similarly, 2PBS, HPBS and 2PSF solid powders were added into tetrahydrofuran solution (concentration of 5×10 -5 M), under ultraviolet light excitation, the solution changes from transparent and colorless to yellow and can be restored. Since the luminescence ability is weak when in solution, but the luminescence performance is significantly enhanced in solid aggregation or high concentration state, after 10s of ultraviolet light irradiation (power is 10W, wavelength is 365nm), blue fluorescence (2PBS compound solid powder and HPBS compound solid powder) and blue-green fluorescence (2PSF compound solid powder) can be clearly seen.
[0118] The 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 were added to tetrahydrofuran solution (concentration of 5×10 -5 M), and then irradiated with ultraviolet light (power of 10 W, wavelength of 365 nm) for different time periods to test its fluorescence spectrum and ultraviolet-visible absorption spectrum; Figure 8 Schematic diagram of the molecular structure changes of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 under ultraviolet light (365 nm);
[0119] Fig. 9The fluorescence spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 under continuous ultraviolet irradiation in tetrahydrofuran change with time; as can be seen from the figure, the fluorescence changes, indicating that the photochromic phenomenon of the molecule is occurring; Fig.10 The UV-visible absorption spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 under continuous UV irradiation in tetrahydrofuran over time; As can be seen from the figure, the UV absorption value increases when the illumination is 3s, indicating that the response speed is fast, and in the UV-visible absorption spectrum, as the illumination time increases, the maximum absorption gradually increases, and when the absorption value reaches the saturation state, the color-changing group in the material is completely or mostly converted into a photoactive form, which involves a photochemical reaction; under the irradiation of ultraviolet light, the structure of the material changes, thereby causing a change in its absorption characteristics; the speed of this process depends on the speed of the photochemical reaction and the intensity of illumination. In the fluorescence spectrum, after the substance absorbs light energy, the electron transitions from the ground state to the excited state, and then returns to the ground state through radiation transition, and the molecule absorbs energy and then transitions from the excited state to the ground state. In addition, the fluorescence intensity depends not only on the generation of the excited state, but also on the fluorescence lifetime, quantum yield and possible non-radiative decay processes.
[0120] The 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 were prepared into tetrahydrofuran solutions (concentration of 5×10 -5 M), and then irradiated with ultraviolet light (power of 10 W, wavelength of 365 nm) for 20 s to test the fluorescence decay curve; Fig.11 The time-resolved fluorescence decay curves of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 are shown in the figure; as can be seen from the figure: the fluorescence lifetimes of the three compounds are 1.02ns, 0.78ns, and 1.17ns, and the fluorescence lifetime refers to the average time required for the fluorescent substance to return to the ground state from the excited state. If the fluorescence lifetime is very short, such as within a few nanoseconds or a shorter time scale, then the fluorescent substance will emit most of the fluorescent photons at the beginning, which is reflected in a higher fluorescence intensity, so it can be seen that the compound emits bright fluorescence. Experimental data and theoretical analysis reveal the general light-induced reversible cyclization and reaction of the benzothiophene involved in the photochromic molecules of the embodiment. The introduction of the benzothiophene group successfully enables these molecules to have significant photochemical activity in addition to the unique photophysical behavior of aggregation-induced emission. The experimental results show that the position and conjugation mode of the benzothiophene group have a significant effect on the color and intensity of the photochromic.
[0121] The 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 were added to a tetrahydrofuran / water mixed solution to obtain a tetrahydrofuran / water solution of the compound (concentration: 5×10-5 M), the volume percentage of water in the tetrahydrofuran / water mixed solution is 0% to 90%, and the volumes of solutions with different water contents are the same; since tetrahydrofuran and water are immiscible in a certain proportion, and the synthesized molecules are also immiscible in aqueous solution, when the water content increases, the organic solvent and the molecules will be squeezed by the water, and when the total volume remains unchanged, the state of the molecules at this time is more aggregated than the state without water, so as to test the fluorescence spectra under different aggregation degrees; Fig.12 The fluorescence spectra of the 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 at different water contents in tetrahydrofuran / water solutions and the fluorescence intensity dotted line graphs are shown; as can be seen from the figures: the prepared molecules are weakly fluorescent or non-fluorescent in pure tetrahydrofuran solution, and as the water content increases from 0% to 90%, the molecules gradually aggregate, and the fluorescence intensity of the molecular solution gradually increases. The drawn dotted line graphs clearly show the rapidly increasing fluorescence intensity, and the typical aggregation-induced emission phenomenon occurs, which solves the fluorescence aggregation-induced quenching (ACQ) problem existing in most traditional photochromic compounds.
[0122] The 2PBS compound, HPBS compound and 2PSF compound prepared in Examples 1 to 3 were added to tetrahydrofuran solution (concentration of 5×10 -5 M), then irradiated under UV light (power of 10 W, wavelength of 365 nm) for 20 s, and then irradiated under visible light (power of 1.5 W, wavelength of 524 nm) for 60 s to perform a photochromic cycle test; Fig.13 The photochromic cycle test graphs of the 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3, which were alternately exposed to ultraviolet light (365 nm) and visible light in a tetrahydrofuran solution; as can be seen from the graph, the compounds exhibited good reversible photochromic stability under 10 cycles of ultraviolet light and visible light in a tetrahydrofuran solution, and could still recover after 10 complete photoswitching cycles, showing excellent cyclability.
[0123] Using different masks, different images were sequentially written on the same filter paper using UV light (power of 10 W, wavelength of 365 nm), and then erased from the same filter paper by exposure to visible light (power of 1.5 W, wavelength of 524 nm). Fig.14This is a photo-controlled patterning application diagram of the reversible photochromic filter paper prepared in Example 4; in the figure, the initial filter paper does not show a pattern. When mask 1 (fennec fox) covers the filter paper and is written with ultraviolet light for 15 seconds, the information of mask 1 appears red, and the written information can be easily removed by itself by exposing it to visible light for 60 seconds. Mask 2 (Northeast Forestry University), mask 3 (cartoon snowman) and mask 4 (snowflake) are used to write and erase alternately. These results show that the prepared compounds can be used as anti-counterfeiting inks and can be used to produce various high-precision optically rewritable patterns.
[0124] The 2PSF@PMMA film prepared in Example 5 and the 2PSF@HPC film prepared in Example 6 were irradiated under ultraviolet light (power of 10 W, wavelength of 365 nm) for 30 s, and then irradiated under visible light (power of 1.5 W, wavelength of 524 nm) for 60 s to perform a photochromic cycle test pattern; Fig.15 The photochromic cycle test diagram of the 2PSF@PMMA film prepared in Example 5 and the 2PSF@HPC film prepared in Example 6 were alternately exposed to ultraviolet light and visible light. It can be seen from the figure that the 2PSF@PMMA and 2PSF@HPC two-component films can undergo multiple cycle experiments under ultraviolet light and visible light cycles, that is, the performance is stable, can be stored and used for a long time, and the material has a long life.
[0125] The 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 were irradiated with ultraviolet light (power of 10 W, wavelength of 365 nm) for different time periods to test their ultraviolet-visible absorption spectra; Fig.16 The UV-visible absorption spectra of 2PBS@HPC / PMMA, HPBS@HPC / PMMA and 2PSF@HPC / PMMA films prepared in Example 7 change with time under continuous UV light irradiation. As can be seen from the figure, the absorption values of 2PBS@HPC / PMMA, HPBS@HPC / PMMA and 2PSF@HPC / PMMA films change with time under continuous UV light irradiation, which gradually increases significantly, indicating that the degree of discoloration of the films deepens.
[0126] The 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 were irradiated under ultraviolet light (power of 10 W, wavelength of 365 nm) for 30 s, and then irradiated under visible light (power of 1.5 W, wavelength of 524 nm) for 60 s to perform a photochromic cycle test; Fig.17The photochromic cycle test diagram of 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 were alternately exposed to ultraviolet light (365nm) and visible light; Fig.13 , 15 It can be seen that the three photochromic molecules 2PBS, HPBS, and 2PSF prepared in Examples 1 to 3 are alternately exposed to ultraviolet light (365nm) and visible light in tetrahydrofuran solution. The photochromic cycle number has good cyclicity in 10 times; Examples 5 and 6 prepare 2PSF@PMMA and 2PSF@HPC two-component films respectively, which are alternately exposed to ultraviolet light (365nm) and visible light for photochromic cycle testing. After 10 complete optical switching cycles, the cyclicity is significantly reduced. The number of cycles between coloring and bleaching of 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA cellulose composite films doubled, and after so many repeated processes, no obvious fatigue was observed in each of them. As a solid matrix, the cellulose composite film can effectively isolate the air from the molecule itself, preventing the free oxygen in the air from affecting the material itself. This fatigue resistance is due to the fact that the cellulose composite film effectively inhibits the oxidation of the molecule by direct contact with free oxygen.
[0127] The 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 were first irradiated with ultraviolet light (power of 10 W, wavelength of 365 nm) for 30 seconds, and then decolorized under natural light. The absorption value after ultraviolet irradiation was tested by a UV-visible spectrophotometer and recorded as 0 seconds. Then, they were spontaneously decolorized under natural light, and the changes in the absorption value were measured by the UV-visible spectrophotometer every one minute. Finally, a curve was drawn according to the measurement results. Fig.18 The relationship curves of the normalized absorbance value and recovery time of the 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7. The results show that the change in absorbance of the sample during the decolorization process is exponentially related to the recovery time. After fitting, the recovery rate constants are 0.003s -1 , 0.012s -1 、0.019s -1 , representing the speed of recovery. In short, the huge variation in bleaching duration also provides a promising strategy for making self-erasing time-dependent information encryption technology.
[0128] The 2PBS@HPC / PMMA, HPBS@HPC / PMMA, and 2PSF@HPC / PMMA films prepared in Example 7 were cut and spliced at different parts to obtain photochromic films based on different isomerization rates. Fig.19 The QR code label based on photochromic films with different isomerization rates prepared in Example 7; it can be seen from the figure that the time-dependent encryption of the QR code information is made by using photochromic films with different decolorization rates. The time-dependent encryption of the QR code can be identified within a specific time range. The change process is divided into four stages: a, b, c and d. Initially, in stage a, all films are transparent and colorless, and the encrypted information cannot be recognized by smart phones. In stage b, after 30 seconds of ultraviolet light irradiation (power of 10W, wavelength of 365nm), the color changes from colorless to yellow. Since the QR code turns yellow, the encrypted QR code cannot be recognized by smart phones. Then, the QR code was placed in visible light (power of 1.5W, wavelength of 524nm) for 120s. Since the fading rate of 2PBS@HPC / PMMA was higher than that of HPBS@HPC / PMMA and 2PSF@HPC / PMMA, the yellow color of the interference part of 2PBS@HPC / PMMA disappeared first, thus inducing the encrypted QR code recognized by the smartphone. The correct encrypted information was "Northeast Forestry University" after scanning the code. This process is stage c. In stage d, when placed in visible light (power of 1.5W, wavelength of 524nm) for 5min, the color of the HPBS@HPC / PMMA part faded further, and the information could not be recognized by the smartphone, achieving the effect of time encryption of the QR code. Due to the different fading rates of each photochromic film, the encrypted QR code can only be recognized within a specific time. Only by knowing the correct encryption method and decryption time can the encrypted information be decrypted.
[0129] Crystal structure analysis is the most effective and direct means to observe molecular stacking. In order to clarify the arrangement of the target molecules 2PBS, HPBS, and 2PSF in the solid state of Examples 1 to 3, crystals were prepared and single crystal XRD experiments were used to analyze the structure of the crystals. The solvent diffusion method was used to grow crystals. The 2PBS compound, HPBS compound, and 2PSF compound prepared in Examples 1 to 3 were dissolved in a good solvent (dichloromethane or tetrahydrofuran) in a test tube, and a small amount of poor solvent (methanol or petroleum ether) was added dropwise. After shaking evenly, the test tube mouth was plugged with cotton, and the test tube was placed in a sealed wide-mouth bottle containing a poor solvent. The same poor solvent was used inside and outside the test tube. The wide-mouth bottle was placed in a crystal incubator with a constant temperature, light-proof, and vibration-proof, and high-quality single crystals could be obtained within a week. Dichloromethane-methanol (volume ratio is 3:1), THF-methanol (volume ratio is 1:1), and dichloromethane-petroleum ether (volume ratio is 3:1) mixed solutions can all grow the same single crystal, and the crystal is a white needle or a regular cube under sunlight.
[0130] Fig. 20 The single crystal structure diagram of 2PBS, HPBS, and 2PSF; Table 1 is the single crystal diffraction data of 2PBS, HPBS, and 2PSF. As can be seen from the diagram, the stacking arrangement structure in the crystal is long-range ordered, and the single crystal XRD experiment can measure the molecular structure and stacking arrangement structure in the crystal. The single crystal XRD experiment measures the crystal system, space group, etc. to which each crystal belongs. Detailed crystal data and refinement data are listed in Table 1.
[0131] Table 1
[0132]
[0133]
Claims
1. A reversible photochromic compound, characterized in that The structural formula of the reversible photochromic compound is 2. The method for preparing a reversible photochromic compound according to claim 1, characterized in that It is carried out in the following steps: The intermediate, the benzothiophene derivative and potassium carbonate are dissolved in a mixed solution of tetrahydrofuran / water, and then tetrakis(triphenylphosphine)palladium is added under nitrogen protection, and the reaction is carried out under condensation reflux for 17h to 48h under a nitrogen atmosphere and a temperature of 60° C. to 90° C. After the reaction is completed, the volatile solvent is removed by reduced pressure distillation, and then the organic phase is extracted three times with ethyl acetate and deionized water, and the organic phase is dried with anhydrous magnesium sulfate. Finally, a mixed solution of dichloromethane / petroleum ether is used as an eluent for column chromatography purification to obtain a reversible photochromic compound; The structural formula of the intermediate is The benzothiophene derivative is benzothiophene-3-boric acid or 3-bromobenzothiophene.
3. The method for preparing a reversible photochromic compound according to claim 2, characterized in that The molar ratio of the intermediate to the benzothiophene derivative is 1:(2-2.6); the molar ratio of the intermediate to potassium carbonate is 1:(2.5-3.5); the molar ratio of the intermediate to tetrakis(triphenylphosphine)palladium is 1:(0.05-0.1); the volume ratio of the molar amount of the intermediate to a mixed solution of tetrahydrofuran / water is 1mmol:(25-35)mL; the volume ratio of tetrahydrofuran to water in the mixed solution of tetrahydrofuran / water is 1:(0.35-0.45); the volume ratio of dichloromethane to petroleum ether in the mixed solution of dichloromethane / petroleum ether is 1:(4-12).
4. The use of the reversible photochromic compound according to claim 1, characterized in that It is used in the preparation of reversible photochromic materials.
5. The use of the reversible photochromic compound according to claim 4, characterized in that The reversible photochromic material changes color under the alternating effects of ultraviolet light and visible light.
6. The use of the reversible photochromic compound according to claim 4, characterized in that The reversible photochromic material is reversible photochromic filter paper, reversible photochromic polymethyl methacrylate film, reversible photochromic hydroxypropyl cellulose film or reversible photochromic cellulose composite film.
7. The use of the reversible photochromic compound according to claim 6, characterized in that When the reversible photochromic material is a reversible photochromic filter paper, it is specifically prepared according to the following steps: The reversible photochromic compound is dissolved in dichloromethane to obtain a transparent solution, the filter paper is immersed in the transparent solution at room temperature for 6 hours to 12 hours, and then dried to obtain the reversible photochromic filter paper; the mass ratio of the filter paper size to the reversible photochromic compound in the transparent solution is 1 cm 2 :(0.5~1)mg; the concentration of the reversible photochromic compound in the transparent solution is 1mol / L~2mol / L.
8. The use of the reversible photochromic compound according to claim 6, characterized in that When the reversible photochromic material is a reversible photochromic polymethyl methacrylate film, it is specifically prepared according to the following steps: Polymethyl methacrylate and a reversible photochromic compound are dissolved in dichloromethane to obtain a transparent solution; the transparent solution is poured into a mold and naturally evaporated and dried at room temperature to obtain a reversible photochromic polymethyl methacrylate film; the mass ratio of the polymethyl methacrylate to the reversible photochromic compound is 1:(0.05-0.2); the mass ratio of the polymethyl methacrylate to the dichloromethane is 1 mg:(0.5-1) mL.
9. The use of the reversible photochromic compound according to claim 6, characterized in that When the reversible photochromic material is a reversible photochromic hydroxypropyl cellulose film, it is specifically prepared according to the following steps: The reversible photochromic compound is dissolved in dimethyl sulfoxide to obtain a transparent solution; hydroxypropyl cellulose is added to distilled water to obtain a hydroxypropyl cellulose aqueous solution; the transparent solution and the hydroxypropyl cellulose aqueous solution are mixed to obtain a mixed solution; the mixed solution is poured into a mold, and heated and dried at a temperature of 60° C. to obtain a reversible photochromic hydroxypropyl cellulose film; the mass ratio of the reversible photochromic compound to the volume of dimethyl sulfoxide is 1 mg: (0.05-0.2) mL; the mass ratio of the hydroxypropyl cellulose to the volume of distilled water is 1 mg: (0.5-1) mL; the mass ratio of the hydroxypropyl cellulose to the reversible photochromic compound in the mixed solution is 1: (0.05-0.25).
10. The use of the reversible photochromic compound according to claim 6, characterized in that When the reversible photochromic material is a reversible photochromic cellulose composite film, it is specifically prepared according to the following steps: The reversible photochromic compound is dissolved in dimethyl sulfoxide to obtain a transparent solution; hydroxypropyl cellulose is added to distilled water to obtain a hydroxypropyl cellulose aqueous solution; the transparent solution is mixed with the hydroxypropyl cellulose aqueous solution to obtain a mixed solution; the mixed solution is poured into a mold covered with a PMMA film, heated and dried at a temperature of 60°C to 65°C, and then the PMMA solution is poured onto the surface, and heated and dried again at a temperature of 60°C to 65°C to form a PMMA / cellulose / PMMA structure, thereby obtaining a reversible photochromic cellulose composite film; The mass ratio of the reversible photochromic compound to dimethyl sulfoxide is 1 mg:(0.05-0.2) mL; the mass ratio of the hydroxypropyl cellulose to distilled water is 1 mg:(0.5-1) mL; the mass ratio of the hydroxypropyl cellulose to the reversible photochromic compound in the mixed solution is 1:(0.05-0.25); the thickness of the single-sided PMMA film is 0.1 mm-0.5 mm; the mass ratio of the single-sided PMMA to the reversible photochromic compound in the reversible photochromic cellulose composite film is 1:(0.1-0.2).
Citation Information
Patent Citations
AIE compound with reversible mechanochromic property and preparation method of the AIE compound
CN110483371A
Piezochromic tetraphenylethylene compound as well as preparation method and application thereof
CN113307727A
Triphenyl vinyl thiophene compound as well as preparation method and application thereof
CN117024401A
Photochromic compound and photoreversible color-developing composition
JP2009079132A