Triarylnaphthyl-containing pyridine imine nickel (II) catalyst and application thereof in polyethylene elastomer synthesis
By using a composite catalytic system of nickel pyridinimine catalyst with triarylnaphthyl and diethylaluminum chloride, the problem of excessive molecular weight of polyethylene elastomer in ethylene polymerization is solved, and the low molecular weight and high polyethylene elastomer are achieved branching degree, meets industrial processing requirements, and demonstrates good mechanical properties.
Patent Information
- Application Number
- CN202410995041.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In the prior art, the weight average molecular weight of the polyethylene elastomer produced by ethylene is a single raw material is too high, resulting in increased difficulty in subsequent processing, and the polyethylene elastomer catalyzed by α-diimine catalysts does not meet the industrial processing requirements.
The catalyst is prepared by a specific synthetic route using a pyridinimine nickel (II) catalyst containing triaryl naphthyl, and a composite catalytic system is formed with the cocatalyst diethylaluminum chloride, which is used for ethylene polymerization, and the reaction temperature and time are controlled to Improve catalytic activity and molecular weight distribution.
The obtained polyethylene elastomer has a reduced molecular weight, high branching degree and good mechanical properties, which meets industrial processing requirements, reduces the difficulty of subsequent processing, and uses iminopyridine nickel catalyst for the first time to prepare polyethylene thermoplastic elastomer.
Smart Images

Figure CN118930589A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of metal catalysis and olefin polymerization, and specifically relates to a pyridine imine nickel (II) catalyst containing triaryl naphthyl and application thereof in the synthesis of polyethylene elastomer. Background Art
[0002] Thermoplastic elastomers show the characteristics of rubber at room temperature, and have excellent elasticity and mechanical properties, so they are used in battery separators, aerospace, communications and other fields. However, in addition to excellent elasticity and mechanical properties, we also have to consider the problem of industrial post-processing. Too high a molecular weight means that its melt index is too low, which increases the difficulty of subsequent processing. The production of polyethylene elastomers with ethylene as the only raw material has cost advantages, but the weight-average molecular weight of polyethylene elastomers produced by α-diimine catalysts is very high, which is not conducive to the post-processing of elastomers.
[0003] CN116789874A discloses an asymmetric large sterically hindered α-diimine nickel catalyst. The weight average molecular weight of the polyethylene elastomer produced by this type of catalyst is much higher than the requirement of industrial processing. Therefore, under the premise of ethylene as the only raw material, the development of a catalyst with high catalytic activity and molecular weight that meets industrial processing conditions can further promote the industrialization of this type of catalyst. Summary of the invention
[0004] In order to overcome the problem of excessive molecular weight of polyethylene elastomer obtained by catalytic polymerization in the prior art, the present invention provides a pyridine imine nickel (II) catalyst containing triaryl naphthyl and its application in the synthesis of polyethylene elastomer. The polyethylene elastomer obtained by this type of catalyst has a lower molecular weight than that obtained by α-diimine catalyst, which is conducive to subsequent processing, and the catalytically synthesized polyethylene material has a high degree of branching, high molecular weight and good mechanical properties such as stretching and recovery, and has good application prospects in the ethylene polymerization preparation industry.
[0005] The triarylnaphthyl-containing pyridine imine nickel (II) catalyst of the present invention has a general structural formula as shown below:
[0006]
[0007] Wherein: R is selected from H, Ph or alkyl; Ar is selected from 3,4,5-substituted phenyl, benzocycloalkyl, thienyl, pyrrolyl, furanyl, naphthyl, benzothienyl or benzofuranyl; X is selected from Cl, Br, Me or alkyl such as ethyl.
[0008] Furthermore, the triarylnaphthyl-containing nickel pyridine imine (II) catalyst of the present invention preferably has the following structure:
[0009]
[0010] Wherein R' is selected from one of H, C1-C6 alkyl and halogen.
[0011] More preferably, R' is selected from one of H(Ni1), Me(Ni2), F(Ni3) and tBu(Ni4).
[0012] Right now:
[0013] Ni1: R=Me, X=Br, R1=H, R2=H, R3=H;
[0014] Ni2: R=Me, X=Br, R1=H, R2=Me, R3=H;
[0015] Ni3: R=Me, X=Br, R1=H, R2=F, R3=H;
[0016] Ni4: R=Me, X=Br, R1=H, R2=tBu, R3=H.
[0017] The synthesis route of the triarylnaphthyl-containing pyridine imine nickel (II) catalyst of the present invention is as follows:
[0018]
[0019] The specific steps include:
[0020] Step 1: Preparation of triaryl naphthyl anilines
[0021] 8-(p-Tolyl)-1-naphthylamine was dissolved in dichloromethane at 0°C, stirred and dispersed evenly, and then N-bromosuccinimide was added in batches, and the reaction was stirred at 0°C for 1.5 hours; during the reaction, a sample was taken every 30 minutes and observed on the thin layer chromatography plate, and the reaction was stopped when a main point appeared on the chromatographic plate; after the reaction was completed, 25 mL of saturated sodium bicarbonate solution was added at 0°C and stirred for 5 minutes, and then the reaction mixture was dissolved in 200 mL of dichloromethane and extracted with 200 mL of water. After extraction three times, anhydrous magnesium sulfate was added to the dichloromethane phase and allowed to stand for 30 minutes, and then the solution was evaporated under reduced pressure to obtain a dark green solid product, and the product was purified by column chromatography (PE:DCM=3:1, V / V) to obtain 2,4-dibromo-8-(p-tolyl)-1-naphthylamine. 2,4-dibromo-8-(p-tolyl)-1-naphthylamine and 4-substituted phenylboronic acid are mixed, and a catalytic amount of tetrakis(triphenylphosphine)palladium and a potassium carbonate aqueous solution are added under a nitrogen atmosphere. The organic phase uses tetrahydrofuran as a solvent and is stirred at 75°C for 24 hours. After the reaction mixture is cooled, the tetrahydrofuran is evaporated under reduced pressure to remove the tetrahydrofuran. The mixture is dissolved in 200 mL of dichloromethane and extracted with 200 mL of water. After three extractions, anhydrous magnesium sulfate is added to the dichloromethane phase and allowed to stand for 30 minutes. The solvent is then evaporated under reduced pressure to obtain a brown-yellow solid. The product is purified by column chromatography (PE:DCM=1:1, V / V) to obtain an intermediate (A1-A4).
[0022] In step 1, the molar ratio of 8-(p-tolyl)-1-naphthylamine to N-bromosuccinimide is 1:2-1:3, and the molar ratio of 2,4-dibromo-8-(p-tolyl)-1-naphthylamine to 4-substituted phenylboronic acid is 1:2.5-1:3.
[0023] Step 2: Preparation of ligand
[0024] The intermediate (A1-A4) prepared in step 1, 2-acetylpyridine and p-toluenesulfonic acid were added to 20 mL of toluene and stirred at 90°C for 24 hours. During the stirring process, samples were taken every 6 hours and observed on the thin layer chromatography plate until a main spot appeared on the thin layer chromatography plate. The solvent was evaporated and concentrated to 5 mL under vacuum, and the remaining solution was diluted with 20 mL of methanol to form a yellow solid, which was filtered, washed with 10 mL of ethanol, and dried under vacuum to obtain ligand compounds (L1-L4) as yellow solid powders.
[0025] In step 2, the molar ratio of the intermediate (A1-A4) to 2-acetylpyridine is 1:0.5-1:5.
[0026] Step 3: Preparation of Catalyst
[0027] Under nitrogen protection, using dichloromethane as solvent, the ligand compounds (L1-L4) and activated nickel bromide (DME) NiBr2 were mixed in a molar ratio of 1:1, and the reaction was stirred at room temperature for 12 hours. The suspension was filtered, the mother liquor was freed from the solvent under vacuum conditions, washed with ether, and dried in vacuum to obtain an orange-red powdery solid, which was the target product.
[0028] The activated nickel bromide (DME) NiBr2 is prepared by the following method:
[0029] Under nitrogen protection, anhydrous nickel bromide is dissolved in anhydrous ethanol, stirred and refluxed until the solution turns dark green, filtered and the filtrate is drained, and then 1,2-dimethoxyethane and triethyl orthoformate solvent (solvent that has been fully stirred and refluxed in advance) are added, refluxed and stirred overnight, and a yellow solid precipitates. The reaction solution is concentrated and the solvent is removed under reduced pressure. After the remaining solvent is cooled, the upper solution is removed, and the resulting product is soaked and washed with 10mL of dry 1,2-dimethoxyethane, and the solvent is removed to obtain an orange-yellow solid powder, which is activated nickel bromide (DME) NiBr2.
[0030] The invention discloses an application of a pyridine imine nickel (II) catalyst containing a triaryl naphthyl group in catalytic synthesis of polyethylene elastomer.
[0031] During the ethylene polymerization process, the catalyst and the co-catalyst diethylaluminum chloride are combined into a composite catalyst system to catalyze the reaction.
[0032] The molar ratio of the catalyst to the co-catalyst diethylaluminum chloride is 1:100-1:2000, preferably 1:100-500, and further preferably 1:200.
[0033] The ethylene polymerization reaction temperature is 0 to 150° C., and the reaction time is 10 to 60 minutes.
[0034] Furthermore, experiments have shown that in the ethylene polymerization reaction, when the reaction temperature is controlled at 10-70°C, the reaction time is 10-30min, and the catalyst dosage is 2μmol, under the activation of the co-catalyst diethylaluminum chloride (Et2AlCl), the catalytic system has a high catalytic activity (up to 10 7 g PE / (mol Ni h), the obtained polyethylene elastomer has a high degree of branching (up to 95 branches / 1000C). The weight average molecular weight of the obtained polyethylene elastomer is effectively reduced, which can meet the requirements of industrial processing.
[0035] The triarylnaphthyl-containing pyridine imine nickel (II) catalyst of the present invention uses 2-acetylpyridine as the catalyst skeleton, and introduces a large sterically hindered triarylnaphthyl imine group into the skeleton, so as to have better heat resistance. The obtained polyethylene material has a high degree of branching, a high molecular weight, and good mechanical properties such as stretching and recovery. The polyethylene elastomer obtained by this type of catalyst has a lower molecular weight than the polyethylene elastomer obtained by the α-diimine catalyst, which is conducive to subsequent processing.
[0036] The beneficial effects of the present invention are embodied in:
[0037] The present invention uses a triarylnaphthyl pyridine nickel catalyst for ethylene polymerization, and the obtained polyethylene elastomer has good mechanical properties and recovery properties, and the weight average molecular weight is effectively reduced, which meets the industrial processing requirements and reduces the difficulty of subsequent processing. Importantly, we use the imino pyridine nickel catalyst for ethylene polymerization to prepare polyethylene thermoplastic elastomer for the first time. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 Figures ad are respectively the tensile curve images of polyethylene prepared by the catalysts of Examples 1 to 4 at 30°C.
[0039] Figure 2 Figures ad are the recovery curve images of polyethylene prepared by the catalysts of Examples 1 to 4 at 30°C.
[0040] Figure 3 The polyethylene prepared by the catalyst of Example 3 at 50°C 1 H NMR and 13 C NMR, where (a) is the 1 HNMR and Figure (b) are for polyethylene 13 C NMR. DETAILED DESCRIPTION
[0041] In order to better understand the technical solution of the present invention, the present invention will be further described in detail below in conjunction with the embodiments. However, it should be understood that these descriptions are only for further illustrating the features and advantages of the present invention, rather than limiting the claims of the present invention.
[0042] Reagents and raw materials used in the examples: All metal organic reactions were carried out under nitrogen protection, and all solvents were dried and deoxygenated. Anhydrous methanol and ethanol were analytically pure and used directly. Toluene was dehydrated by molecular sieve, refluxed with sodium metal under nitrogen protection, and evaporated before use.
[0043] Embodiment 1:
[0044] 1. Synthesis of 2,4-dibromo-8-(p-tolyl)-1-naphthylamine
[0045] 8-(p-Tolyl)-1-naphthylamine (20.0mmol, 1.0 equivalent) was dissolved in 20mL dichloromethane at 0°C and stirred, N-bromosuccinimide (40.0mmol, 2.0 equivalent) was added in batches, and the reaction was stirred at 0°C for 1.5h. During the reaction, samples were taken every 30min and observed on the thin layer chromatography plate. The reaction stopped when a main point appeared on the chromatographic plate. After the reaction was completed, 25mL of saturated sodium bicarbonate solution was added at 0°C and stirred for 5 minutes, then the reaction mixture was dissolved in 200mL of dichloromethane solution, extracted with 200mL of water, extracted three times, anhydrous magnesium sulfate was added to the dichloromethane phase and allowed to stand for 30 minutes, then the solution was evaporated under reduced pressure to obtain a dark green solid product, and the product was purified by column chromatography (PE:DCM=3:1) with a yield of 63%. The synthetic route is shown below:
[0046]
[0047] NMR analysis: 1 H NMR (400MHz, CDCl3) δ8.21 (d, J=8.4Hz, 1H, Ar-H), 7.84 (s, 1H, Ar-H), 7.50 (dd, J=8.5, 7.1Hz, 1H, Ar- H),7.28(d,J=8.4Hz,3H,Ar-H),7.23(d,J=7.4Hz,2H,Ar-H),4.43(s,2H,-NH2),2.44(s,3H,Ar-CH3). 13 C NMR (101MHz, CDCl3) δ141.15,139.48,138.74,137.95,133.34,132.64,130.1 3,129.24,129.16,127.90,126.32,121.79,110.02,104.39,21.40(Ar-CH3).
[0048] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 17 H 14 Br2N + :391.9468,Found,391.9460,[M+H] +
[0049] 2. Synthesis of triarylnaphthylarylamine (A1)
[0050] 2,4-dibromo-8-(p-tolyl)-1-naphthylamine (1.5mmol, 1.0 equivalent) and phenylboronic acid (3.0mmol, 2.0 equivalent) were mixed, and a catalytic amount of tetrakis(triphenylphosphine)palladium and an aqueous solution of potassium carbonate (7.5mmol, 5.0 equivalent) were added under a nitrogen atmosphere. The organic phase was stirred at 75°C with tetrahydrofuran as the solvent for 24 hours. After the reaction mixture was cooled, the tetrahydrofuran was evaporated under reduced pressure to remove the tetrahydrofuran. The mixture was dissolved in 200mL of dichloromethane and extracted with 200mL of water. After three extractions, anhydrous magnesium sulfate was added to the dichloromethane phase and allowed to stand for 30 minutes. The solvent was then evaporated under reduced pressure to obtain a brown-yellow aromatic amine A1 solid. The product was purified by column chromatography (PE:DCM=1:1) with a yield of 86%. The synthetic route is as follows:
[0051]
[0052] NMR analysis: 1 H NMR (400MHz, CDCl3) δ7.94 (d, J=8.5Hz, 1H, Ar-H), 7.55-7.34 (m, 12H, Ar-H), 7.32-7.28 ( m,2H,Ar-H),7.23(dd,J=13.8,5.2Hz,3H,Ar-H),4.08(s,2H,-NH2),2.43(s,3H,Ar-CH3). 13 C NMR (101MHz, CDCl3) δ141.69,140.95,140.23,140.13,138.82,137.10,133.16,130.52,130.07,129.80,1 29.06,128.91,128.85,128.77,128.17,127.04,126.57,126.42,124.60,122.10,120.71,21.19(Ar-CH3).
[0053] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 29 H 24 N + :386.1904,Found,386.1901,[M+H] +
[0054] 3. Synthesis of catalyst ligand (L1)
[0055] A1 (1.0 mmol, 1.0 equivalent), 2-acetylpyridine (1.0 mmol, 1.0 equivalent) and p-toluenesulfonic acid (20 mg) were added to toluene (20 mL) and stirred at 90 ° C for 24 hours. During the stirring process, samples were taken every 6 hours and observed on the thin layer chromatography plate until a main spot appeared on the thin layer chromatography plate. The solvent was evaporated and concentrated to 5 mL under vacuum. The remaining solution was diluted with methanol (20 mL) to form a yellow solid, which was filtered and washed with 10 mL of ethanol. After vacuum drying, a yellow solid powder (L1) was obtained with a yield of 83%. The synthetic route is shown below:
[0056]
[0057] Mass spectrometry: ACPI-MS:calcd for C 36 H 29 N2 + :489.2326,Found,489.2317,[M+H] +
[0058] 4. Synthesis of Catalyst Ni1
[0059] Ni1 complex was synthesized by reacting (DME)NiBr2 (DME = 1,2-dimethoxyethane) with the corresponding ligand in dichloromethane. In a nitrogen atmosphere, 0.2mmol of ligand L1 was dissolved in 10mL of dichloromethane, and then activated (DME)NiBr2 (0.2mmol, 62mg) was added to the above solution, and the resulting mixture was stirred at room temperature overnight. Most of the solvent was removed by evaporation under reduced pressure, washed with 4×5mL of ether, filtered, and vacuum dried to obtain an orange-red solid product Ni1 with a yield of 90%. The synthesis route is as follows:
[0060]
[0061] Mass spectrometry: ACPI-MS:calcd for C 36 H 28 BrN2Ni:625.0789,Found,625.0784,[M+H] +
[0062] Embodiment 2:
[0063] 1. Synthesis of triaryl naphthyl aromatic amine (A2)
[0064] The phenylboric acid in step 2 of Example 1 was replaced with p-methylphenylboric acid, and the remaining operations were the same as those in step 2 of Example 1, with a yield of 84%.
[0065] NMR analysis: 1H NMR (400MHz, CDCl3) δ7.95 (d, J=8.3Hz, 1H, Ar-H), 7.43-7.31 (m, 7H, Ar-H), 7.29 (d, J=9.0Hz, 2H, Ar-H) ,7.26-7.18(m,6H,Ar-H),4.06(s,2H,-NH2),2.45(s,3H,-CH3),2.42(s,3H,-CH3),2.36(s,3H,-CH3). 13 C NMR (101MHz, CDCl3) δ136.63,135.59,134.36,132.84,132.61,132.24,131.72,128.76,125.97,125.69,125.58,1 25.23,125.10,124.65,124.47,124.43,124.32,122.07,120.00,117.74,116.33,16.79(Ar-CH3),16.74(Ar-CH3).
[0066] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 31 H 28 N + :414.2217,Found,414.2209,[M+H] +
[0067] 2. Synthesis of catalyst ligand (L2)
[0068] A1 in step 3 of Example 1 was replaced by A2, and the remaining operations were the same as step 3 of Example 1, with a yield of 80%.
[0069] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 38 H 33 N2 + :517.2639,Found,517.2637,[M+H] +
[0070] 3. Synthesis of Catalyst Ni2
[0071] L1 in step 4 of Example 1 was replaced by L2, and the remaining operations were the same as step 4 of Example 1, with a yield of 93%.
[0072] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 38 H 32 BrN2Ni:653.1102,Found,653.1097,[M+H] +Embodiment 3:
[0073] 1. Synthesis of triarylnaphthylarylamine (A3)
[0074] The phenylboric acid in step 2 of Example 1 was replaced with 4-fluorophenylboric acid, and the remaining operations were the same as those in step 2 of Example 1, with a yield of 81%.
[0075] NMR analysis: 1 H NMR (400MHz, CDCl3) δ7.85 (d, J = 8.5Hz, 1H, Ar-H), 7.48-7.35 (m, 7H, Ar-H), 7.26-7.08 (m, 8H, Ar-H), 4.03 (s, 2H, -NH2), 2.43 (s, 3H, -CH3). 13 C NMR(101MHz,CDCl3)δ163.17(CF),163.14(CF),160.71(CF),160.70(CF),14 0.74,140.41,138.90,137.50,137.47,137.25,136.00,135.96,133.30,131. 95,131.88,131.52,131.45,129.98,129.06,129.04,128.98,128.83,126.1 9,124.84,120.92,120.69,115.89,115.68,115.17,114.96,21.20(Ar-CH3).
[0076] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 29 H 22 F2N + :422.1715,Found,422.1707,[M+H] +
[0077] 2. Synthesis of catalyst ligand (L3)
[0078] A1 in step 3 of Example 1 was replaced by A3, and the remaining operations were the same as step 3 of Example 1, with a yield of 85%.
[0079] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 36 H 27 F2N2 + :525.2137,Found,525.2134,[M+H] +
[0080] 3. Synthesis of Catalyst Ni3
[0081] L1 in step 4 of Example 1 was replaced by L3, and the remaining operations were the same as step 4 of Example 1, with a yield of 95%.
[0082] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 36 H 26 BrF2N2Ni:661.0601,Found,661.0595,[M+H] + Embodiment 4:
[0083] 1. Synthesis of triarylnaphthylarylamine (A4)
[0084] The phenylboric acid in step 2 of Example 1 was replaced with 4-tert-butylphenylboric acid, and the remaining operations were the same as step 2 of Example 1, with a yield of 82%.
[0085] NMR analysis: 1 H NMR (400MHz, CDCl3) δ8.01 (d, J=8.5, 1.4Hz, 1H, Ar-H), 7.51-7.32 (m, 12H, Ar-H), 7.26-7.20 (m,3H,Ar-H),4.08(s,2H,-NH2),2.43(s,3H,Ar-CH3),1.43(s,9H,-CH3),1.35(s,9H,-CH3). 13 C NMR (101MHz, CDCl3) δ149.84,149.30,141.08,140.00,138.74,138.69,13 7.21,137.00,133.13,130.18,130.12,129.96,129.41,129.08,128.79,1 28.71,126.58,125.70,125.05,124.38,122.20,120.75,34.53(-C(CH3)3 ),34.50(-C(CH3)3),31.47(-C(CH3)3),31.33(-C(CH3)3),21.19(-CH3).
[0086] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 37 H 40 N + :498.3156,Found,498.3152,[M+H] +
[0087] 2. Synthesis of catalyst ligand (L4)
[0088] A1 in step 3 of Example 1 was replaced by A4, and the remaining operations were the same as step 3 of Example 1, with a yield of 84%.
[0089] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 44 H 45 N2 + :601.3578,Found,601.3563,[M+H] +
[0090] 3. Synthesis of Catalyst Ni4
[0091] L1 in step 4 of Example 1 was replaced by L4, and the remaining operations were the same as step 4 of Example 1, with a yield of 92%.
[0092] Mass spectrometry analysis: ACPI-MS (m / z):calcd for C 44 H 44 BrN2Ni:737.2041,Found,737.2036,[M+H] +
[0093] Example 5: Application of Ni1-Ni4 in catalytic ethylene polymerization
[0094] First, place a 350mL thick-walled pressure-resistant bottle with a magnet in an oven at 100°C for 6 hours, and bring it into a glove box by replacing nitrogen. Then, add 40mL of toluene to the pressure-resistant bottle, take it out, connect it to a high-pressure gas pipeline with ethylene gas, and raise the temperature to the required temperature. At the same time, turn on the vacuum pump to evacuate the polymerization gas pipeline, and turn off the vacuum pump after 3 minutes. Ethylene is introduced, and the catalyst nickel complex (2.0μmol) and diethylaluminum chloride (400μmol) dissolved in 2mL of dichloromethane are injected into the polymerization pressure-resistant bottle with a syringe under an ethylene atmosphere, and the pressure reducing valve is slowly adjusted to increase to the required polymerization pressure and maintain, and the time is recorded. Finally, the polymerization reaction is terminated, and a large amount of 5% (volume) acidified anhydrous ethanol is added, the polymer is precipitated, filtered, washed with anhydrous ethanol several times, and dried in a vacuum drying oven at 60°C for 24 hours.
[0095] The following table shows the experimental conditions for ethylene polymerization using the catalyst provided by the present invention, as well as the catalyst (Cat.), temperature (T), yield (Yield), catalytic activity (Act.), polymer molecular weight (M n ), polymer molecular weight distribution (PDI), degree of branching (brs) and other polymerization result data.
[0096] Table 1 Ethylene polymerization
[0097]
[0098]
[0099] a Polymerization conditions: catalyst 2.0 μmol, dichloromethane = 2 mL, [Al] / [Ni] = 200, n-heptane = 40 mL, ethylene pressure 6 atm, time = 10 min;
[0100] b The unit of activity is 10 7 g mol -1 h -1 ;
[0101] c Polymer molecular weight M n and molecular weight distribution PDI were determined by gel permeation chromatography (GPC) at 150 °C in trichlorobenzene and polystyrene standards;
[0102] d The degree of branching refers to the number of branches per 1000 carbon atoms, which is 1 H NMR nuclear magnetic resonance determination;
[0103] e Melting point m Determined by differential scanning calorimetry (DSC).
[0104] As shown in Table 1, the Ni1-Ni4 catalysts prepared by the present invention can catalyze the preparation of polyethylene with high activity, and the molecular weight of the prepared polymer can reach 10 7 g / mol) and branching degree (up to 95 branches / 1000C), and the polymer is a thermoplastic elastomer. Through mechanical property testing of polyethylene, it was found that the polyethylene prepared by the catalyst of this system at 30°C has good mechanical properties and recovery performance, with a recovery rate of up to 85%, moderate tensile strength and good recovery performance. At the same time, its weight-average molecular weight meets the requirements of industrial post-processing, and has good application prospects in the olefin polymerization industry. Importantly, we used the iminopyridine nickel catalyst for the first time to prepare polyethylene elastomers with ethylene polymerization.
[0105] The above is a detailed introduction to a preferred compound, complex catalyst, catalyst composition and method for preparing an olefin polymer provided by the present invention. Specific examples are used herein to illustrate the principles and implementation methods of the present invention, but the present invention is not limited to the specific implementation methods described herein. It is understood by those skilled in the art that other changes and modifications may be made without departing from the scope of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A nickel pyridine imine (II) catalyst containing a triaryl naphthyl group, characterized in that Its general structure is shown below: Wherein: R is selected from H, Ph or alkyl; Ar is selected from 3,4,5-substituted phenyl, benzocycloalkyl, thienyl, pyrrolyl, furanyl, naphthyl, benzothienyl or benzofuranyl; X is selected from Cl, Br or alkyl.
2. The triarylnaphthyl-containing pyridine imine nickel (II) catalyst according to claim 1, characterized in that Its general structure is shown below: Wherein R' is selected from one of H, C1-C6 alkyl and halogen.
3. The triarylnaphthyl-containing pyridine imine nickel (II) catalyst according to claim 2, characterized in that: R' is selected from one of H, Me, F and tBu.
4. The method for preparing the triarylnaphthyl-containing pyridine imine nickel (II) catalyst according to claim 3, characterized in that Its synthetic route is as follows:
5. The preparation method according to claim 4, characterized in that The following steps are involved: Step 1: Preparation of triaryl naphthyl anilines 8-(p-tolyl)-1-naphthylamine is dissolved in dichloromethane at 0°C, stirred and dispersed evenly, then N-bromosuccinimide is added in batches, and stirred and reacted at 0°C; after the reaction is completed, separation and purification are performed to obtain 2,4-dibromo-8-(p-tolyl)-1-naphthylamine; 2,4-dibromo-8-(p-tolyl)-1-naphthylamine and 4-substituted phenylboronic acid are mixed, and a catalytic amount of tetrakis(triphenylphosphine)palladium and a potassium carbonate aqueous solution are added under a nitrogen atmosphere, and the organic phase is stirred and reacted at 75°C using tetrahydrofuran as a solvent. After the reaction is completed, separation and purification are performed to obtain an intermediate; Step 2: Preparation of ligand The intermediate prepared in step 1, 2-acetylpyridine and p-toluenesulfonic acid are added to toluene, and the mixture is stirred at 90° C. to react; after the reaction is completed, the solvent is evaporated, and the mixture is concentrated in vacuo, and the remaining solution is diluted with methanol to form a yellow solid, which is filtered, washed with ethanol, and dried in vacuo to obtain a ligand compound; Step 3: Preparation of Catalyst Under nitrogen protection, using dichloromethane as solvent, the ligand compound prepared in step 2 was mixed with activated nickel bromide (DME) NiBr2 in a molar ratio of 1:1, and the reaction was stirred at room temperature for 12 hours. The suspension was filtered, the mother liquor was freed from the solvent under vacuum conditions, washed with ether, and dried in vacuum to obtain an orange-red powdery solid, which was the target product.
6. The preparation method according to claim 5, characterized in that The activated nickel bromide (DME) NiBr2 is prepared by the following method: Under nitrogen protection, anhydrous nickel bromide is dissolved in anhydrous ethanol, stirred and refluxed until the solution turns dark green. After filtering, the filtrate is drained, and 1,2-dimethoxyethane and triethyl orthoformate solvents are added, refluxed and stirred for 8-12 hours, and a yellow solid precipitates. The reaction solution is concentrated, and the solvent is removed under reduced pressure. After the remaining solvent is cooled, the upper solution is removed, and the obtained product is soaked and washed with dry 1,2-dimethoxyethane, and the solvent is removed to obtain an orange-yellow solid powder, which is activated nickel bromide (DME) NiBr2.
7. Use of the triarylnaphthyl-containing pyridine imine nickel (II) catalyst according to claim 1 in the catalytic synthesis of polyethylene elastomers.
8. The use according to claim 7, characterized in that: During the ethylene polymerization process, the catalyst and the co-catalyst diethylaluminum chloride are combined into a composite catalyst system for catalytic reaction.
9. The use according to claim 8, characterized in that: The molar ratio of the catalyst to the co-catalyst diethylaluminum chloride is 1:100-1:2000.
10. The use according to claim 7, characterized in that: The ethylene polymerization reaction temperature is 0 to 150° C., and the reaction time is 10 to 60 minutes.