Fluorine-containing polymer, conductive paste, negative electrode sheet, secondary battery, and electric device
By using fluoropolymers to improve the dispersibility and anti-gelling properties of conductive slurry, the problems of electrode cold pressing rebound and slurry gelation were solved, thereby improving electrode quality and battery performance.
Patent Information
- Application Number
- CN202310534845.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-12
AI Technical Summary
In existing technologies, secondary battery electrodes are prone to rebound during cold pressing, which affects battery assembly processes and electrochemical performance. Furthermore, conductive slurry is prone to gelation during storage, leading to a decline in battery performance.
Fluoropolymers are used as dispersants to prepare fluoropolymers through polymerization reactions. These fluoropolymers are used to improve the dispersibility and anti-gelling properties of conductive slurries, increase the cohesion of electrode sheets, reduce electrode rebound rate, and reduce the DC internal resistance of batteries.
It improves the cohesiveness of the electrode, reduces the rebound rate after cold pressing, improves the dynamic performance and storage stability of the battery, and reduces the DC internal resistance and film resistance of the battery.
Smart Images

Figure CN118930706A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of secondary batteries, and in particular to a fluorine-containing polymer, a conductive slurry, a negative electrode sheet, a secondary battery and an electrical device. Background Art
[0002] Secondary batteries have many advantages such as high volumetric and mass energy density, long cycle life, high nominal voltage, low self-discharge rate, small size and light weight, and are widely used in the field of consumer electronics.
[0003] The preparation of secondary batteries requires multiple processes, including cold pressing of pole pieces, pole piece die cutting, assembly, baking, and liquid injection. Pole piece manufacturing belongs to the front-end process and occupies an important position in the whole process. The quality of pole pieces is related to the progress of the middle-stage assembly process of secondary batteries, and also affects the electrochemical performance of the back-end and secondary batteries. Summary of the invention
[0004] The present application is made in view of the above-mentioned problems, and its purpose is to provide a fluorine-containing polymer and a conductive paste containing the fluorine-containing polymer, which can improve the cohesive force of the electrode, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the use quality of the electrode while improving the dispersibility of the conductive paste and slowing down the gel of the conductive paste.
[0005] The first aspect of the present application provides a fluorine-containing polymer, comprising at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II,
[0006]
[0007] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOM, M is selected from hydrogen, NH4 or alkali metal.
[0008] On the one hand, the fluorine-containing polymer provided in the present application can act as a dispersant, which can significantly alleviate the gelation of the conductive slurry during the storage process, improve the anti-gelation and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery. On the other hand, the fluorine-containing polymer can increase the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode.
[0009] In any embodiment, M comprises one or more of lithium, sodium, and potassium.
[0010] The lithium, sodium or potassium introduced into the fluorinated polymer can form ion exchange with the active ions during the charge and discharge process, further increasing the mobility of the active ions, reducing the DC internal resistance of the battery, and improving the kinetic performance of the battery.
[0011] In any embodiment, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0012] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of all structural units in the fluorine-containing polymer.
[0013] By controlling the molar content of the structural unit derived from the monomer represented by Formula I within a suitable range, the viscosity of the conductive paste, the cohesive force of the pole piece, and the rebound rate of the pole piece after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0014] In any embodiment, the molar content of the structural unit derived from the monomer represented by formula II is 20% to 40%, based on the total molar number of all structural units in the fluorine-containing polymer.
[0015] By controlling the molar content of the structural unit derived from the monomer represented by Formula II within a suitable range, the viscosity of the conductive paste, the cohesive force of the pole piece and the rebound rate of the pole piece after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0016] In any embodiment, the weight average molecular weight of the fluorine-containing polymer is 80,000 to 120,000.
[0017] By controlling the weight average molecular weight of the fluorine-containing polymer within a suitable range, the viscosity of the conductive paste, the cohesive force of the pole piece and the rebound rate of the pole piece after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0018] In any embodiment, the monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0019] In any embodiment, the monomer shown in Formula II is selected from allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioic acid, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioic acid, lithium maleic acid, trans-lithium glutaconedioic acid, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octadecene, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleic acid, trans-sodium glutaconedioic acid, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octadecene, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
[0020] In any embodiment, the fluorine-containing polymer includes one or more of vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butylmalonate copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-chlorotrifluoroethylene-allyl lithium malonate copolymer, tetrafluoroethylene-allyl lithium propylene copolymer, and vinylidene fluoride-hexafluoropropylene-allyl lithium propylene copolymer.
[0021] The second aspect of the present application provides a method for preparing a fluorine-containing polymer, comprising the following steps:
[0022] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0023]
[0024] Wherein, R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, wherein R4, R5, R6 and R7 contain at least two -COOH groups,
[0025] Optionally, the polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least a portion of -COOH in the polymer product into -COOM, where M is selected from NH4 or an alkali metal.
[0026] Compared with traditional dispersants, the fluorine-containing polymer prepared by this method can not only improve the dispersibility of the conductive slurry, alleviate the gelation of the conductive slurry during storage, improve the anti-gelation and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and improve the dynamic performance of the battery, but the fluorine-containing polymer can also improve the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode.
[0027] In any embodiment, M comprises one or more of lithium, sodium, and potassium.
[0028] In any embodiment, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0029] In any embodiment, the molar content of the monomer represented by formula I is 60%-80%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0030] In any embodiment, the molar content of the monomer represented by formula II is 20%-40%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.
[0031] In any embodiment, the polymerization reaction specifically comprises:
[0032] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0033] Second stage polymerization: after a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization;
[0034] Optionally, after the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0035] The method provided in the present application forms a fluorine-containing segment by first continuously feeding the monomer shown in formula I, so that the fluorine-containing polymer has high thermal stability; and then the monomer shown in formula II is introduced to reduce the contact between the fluorine-containing segment and the external environment, effectively alleviating the gel phenomenon caused by the fluorine element. Compared with the fluorine-containing polymer prepared by simultaneously polymerizing by passing all the monomers into the reaction vessel, the fluorine-containing polymer prepared by this method can effectively improve the stability of the conductive slurry, improve the dispersibility of the slurry, reduce the diaphragm resistance of the pole piece and the DC internal resistance of the battery, and improve the dynamic performance of the battery. In addition, when the monomer shown in formula II is fed into the reaction vessel for the second stage of polymerization reaction, the monomer shown in formula I is continuously fed into the reaction vessel, which helps to improve the compatibility of the segment generated by the first stage of polymerization reaction with the segment generated by the second stage of polymerization reaction, and improve the stability of the fluorine-containing polymer.
[0036] In any embodiment, the mass of the monomer of formula I introduced in the first stage polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0037] In any embodiment, the neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia water.
[0038] The third aspect of the present application provides use of the fluorine-containing polymer of the first aspect in a secondary battery.
[0039] In a fourth aspect of the present application, a conductive paste is provided, comprising a conductive agent, an aqueous medium and the fluorine-containing polymer described in the first aspect.
[0040] Compared with the prior art of directly adding a conductive agent during the preparation of the negative electrode slurry, the conductive slurry provided in the present application can reduce the rebound rate of the electrode after cold pressing for 24 hours, thereby improving the quality of the electrode. At the same time, by improving the dispersibility of the conductive agent in the negative electrode slurry, the conductive effect of the conductive agent in the electrode is improved, thereby effectively reducing the conductive agent content in the electrode, which is beneficial to further increase the loading amount of the negative electrode active material in the electrode and improve the battery power performance.
[0041] In any embodiment, the mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste.
[0042] The mass fraction of the conductive agent is controlled within a suitable range. Based on the total mass of the conductive slurry, the slurry has a suitable viscosity. At the same time, the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the slurry.
[0043] In any embodiment, the mass fraction of the fluorine-containing polymer is 0.5%-1.5%, based on the total mass of the conductive paste.
[0044] By controlling the mass fraction of the fluorine-containing polymer within a suitable range, the slurry has a suitable viscosity based on the total mass of the conductive slurry, and the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the slurry.
[0045] In any embodiment, the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500 mPa·s-5000 mPa·s.
[0046] The solid content is 1%-10%, and the viscosity is 500mPa·s-5000mPa·s. It can be directly mixed and stirred with active materials and binders to prepare negative electrode slurry without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.
[0047] The fifth aspect of the present application provides a negative electrode plate, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry of the fourth aspect.
[0048] Compared with the negative electrode plates prepared by directly adding conductive agent powder in the prior art, the conductive agent in the negative electrode plates disclosed in the present application exists in the negative electrode plates in the form of conductive slurry deposits. On the one hand, the cohesion of the plates can be improved, the rebound rate of the plates after cold pressing for 24 hours can be reduced, and the quality of the plates can be improved. On the other hand, adding the conductive slurry can improve the dispersion performance of the conductive material, so that the negative electrode plates can have low membrane resistance when the conductive agent is added in a low amount, which provides the possibility of further increasing the loading amount of the negative electrode active material in the plates.
[0049] In any embodiment, the compaction density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode plate is cold pressed for 24 hours, the plate rebound rate is not higher than 7.0%.
[0050] In any embodiment, the cohesive force of the negative electrode plate is not less than 73 N / m, and can be optionally not less than 80 N / m.
[0051] In any embodiment, based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the film resistance of the negative electrode film layer is not higher than 0.15Ω.
[0052] A sixth aspect of the present application provides a secondary battery, characterized in that it includes the negative electrode sheet of the fifth aspect.
[0053] In any embodiment, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0054] A seventh aspect of the present application provides an electrical device comprising the secondary battery of the sixth aspect. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0056] Figure 2 yes Figure 1 An exploded view of a secondary battery according to an embodiment of the present application is shown;
[0057] Figure 3 is a schematic diagram of a battery module according to an embodiment of the present application;
[0058] Figure 4is a schematic diagram of a battery pack according to an embodiment of the present application;
[0059] Figure 5 yes Figure 4 An exploded view of a battery pack according to an embodiment of the present application is shown;
[0060] Figure 6 FIG. 1 is a schematic diagram of an electric device using a secondary battery according to an embodiment of the present application as a power source.
[0061] Description of reference numerals:
[0062] 1 battery pack; 2 upper box; 3 lower box; 4 battery module; 5 secondary battery; 51 shell; 52 electrode assembly; 53 cover plate. DETAILED DESCRIPTION
[0063] Hereinafter, the embodiments of the fluorinated polymer, conductive paste, negative electrode plate, secondary battery and electric device of the present application are specifically disclosed with appropriate reference to the accompanying drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structures are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0064] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0065] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0066] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0067] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0068] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0069] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).
[0070] As the energy density of secondary batteries gradually increases, battery manufacturers increase the compaction density of pole pieces so that more pole pieces can be loaded into the limited shell volume, thereby achieving the purpose of increasing the energy density of the battery cell. However, in the actual production process of pole pieces, as the compaction density of pole pieces increases, the cold pressing process will cause damage to the active material, there will be insufficient gaps between particles, the internal repulsive force is too large, and the pole pieces are prone to increase in thickness after cold pressing, and the pole pieces will rebound, affecting the subsequent battery assembly process.
[0071] [Fluoropolymer]
[0072] Based on this, the present application proposes a fluorine-containing polymer, comprising at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II.
[0073]
[0074] Wherein, R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOM, M is selected from hydrogen, NH4 or alkali metal.
[0075] As used herein, the term "fluorine-containing polymer" refers to a polymer containing fluorine in its structural units.
[0076] In this context, the term "polymer" includes, on the one hand, a collection of macromolecules that are chemically uniform but differ in degree of polymerization, molar mass and chain length, prepared by polymerization. The term also includes, on the other hand, derivatives of such a collection of macromolecules formed by polymerization, i.e. products that can be obtained by reaction of functional groups in the above-mentioned macromolecules, such as addition or substitution, and can be chemically uniform or chemically inhomogeneous.
[0077] In this article, the term “C 1-3 "Alkyl" refers to both branched and straight-chain saturated aliphatic monovalent hydrocarbon radicals having the specified number of carbon atoms, no unsaturation present in the radical, having from one to three carbon atoms, and attached to the rest of the molecule by a single bond.
[0078] In this context, the term “C 1-3 "Alkyl" refers to an alkyl group containing 1-3 C in which at least one H atom is replaced by a F atom. In some embodiments, a C 1-3 The alkyl group includes a -CF3 group and a -C2F6 group.
[0079] In this article, the term “C 1-15 "Alkyl" refers to both branched and straight-chain saturated aliphatic monovalent hydrocarbon radicals having the specified number of carbon atoms, with no unsaturation present in the radical, having from one to fifteen carbon atoms, and attached to the rest of the molecule by a single bond.
[0080] As used herein, the term "substituted" means that at least one hydrogen atom of the compound or chemical moiety is replaced by another chemical moiety with a substituent, wherein each substituent is independently selected from the group consisting of: hydroxyl, thiol, amino, cyano, nitro, aldehyde, halogen, alkenyl, alkynyl, aryl, heteroaryl, C 1-6 Alkyl, C 1-6 Alkoxy.
[0081] In some embodiments, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0082] As used herein, the term "alkali metals" refers to the six metal elements in Group IA of the periodic table except hydrogen (H), namely lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr).
[0083] In some embodiments, -COOM includes any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0084] In some embodiments, R4, R5, R6 and R7 contain at least two -COOH groups.
[0085] In some embodiments, R4, R5, R6 and R7 contain at least two -COO NH4.
[0086] In some embodiments, R4, R5, R6 and R7 contain at least two -COOLi.
[0087] In some embodiments, R4, R5, R6 and R7 contain at least two -COONa.
[0088] In some embodiments, R4, R5, R6 and R7 contain at least two -COOKs.
[0089] In some embodiments, R4, R5, R6 and R7 independently include any two or more of -COOH, -COONH4, -COOLi, -COONa, -COOK.
[0090] In some embodiments, R4 and R5 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0091] In some embodiments, in some embodiments, R6 and R7 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0092] In some embodiments, R4 and R6 are independently selected from any one of -COOH, -COONH4, -COOLi, -COONa, and -COOK.
[0093] In some embodiments, R4 contains two or more -COOH, -COONH4, -COOLi, -COONa or -COOK.
[0094] In some embodiments, the monomer represented by formula I is selected from one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene, and hexafluoropropylene.
[0095] In some embodiments, the monomer represented by formula II is selected from the group consisting of allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioic acid, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioic acid, lithium maleic acid, trans-glutaconedioic acid, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octadecene, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleic acid, trans-glutaconedioic acid, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octadecene, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
[0096] In this article, the term "process window" refers to the process range that can ensure product quality, including but not limited to temperature range, pressure range, storage time length, etc. It can be understood that the wider the process window, the lower the requirement for process accuracy.
[0097] As used herein, the term "carboxylate group" refers to -COONH4, -COOLi, -COONa, -COOK, -COORb, -COOCs, -COOFr.
[0098] In some embodiments, the polymer comprises one or more structural units derived from the monomers shown in formula I. In some embodiments, the polymer comprises one or more structural units derived from the monomers shown in formula II. In some embodiments, the polymer includes but is not limited to fluorine-containing polymers including vinylidene fluoride-allyl dilithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butyl malonate copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-chlorotrifluoroethylene-lithium allyl malonate copolymer, hexafluoropropylene-sodium vinyl malonate copolymer.
[0099] The fluorine element in the structural unit derived from the monomer shown in formula I can form hydrogen bonds with the hydroxyl group or / and carboxyl group on the surface of the active substance. In addition, the carboxyl group and / or carboxylate group contained in the structural unit derived from the monomer shown in formula II can form hydrogen bonds with the hydroxyl group or / and carboxyl group on the surface of the active substance. The two work together to improve the cohesion of the pole piece, reduce the irreversible expansion of the pole piece during the manufacturing process, reduce the rebound rate of the pole piece after cold pressing for 24 hours, and improve the quality of the pole piece. In addition, the structural unit derived from the monomer shown in formula II can effectively reduce the fluorine content of the fluorine-containing polymer and improve the slurry gel phenomenon caused by the fluorine element. Moreover, the structural unit derived from the monomer shown in formula II can further increase the steric hindrance of the fluorine-containing polymer, reduce the aggregation of the fluorine-containing unit, play a role in reducing the viscosity of the slurry, alleviate the gel of the slurry, and effectively improve the filterability of the slurry. The structural unit derived from the monomer shown in Formula II contains at least two carboxyl groups and / or carboxylate groups, which can further improve the cohesion of the electrode and reduce the rebound rate of the electrode after cold pressing. In addition, it can also reduce the viscosity of the conductive paste and improve the filterability of the conductive paste, making it less likely for the conductive paste to gel during storage, thereby improving the anti-gelling and storage properties of the conductive paste and further reducing the DC impedance of the battery.
[0100] In summary, the fluorine-containing polymer provided in the present application can, on the one hand, act as a dispersant, which can significantly alleviate the gelation of the conductive slurry during storage, improve the anti-gelation and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery; on the other hand, the fluorine-containing polymer can increase the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode.
[0101] In some embodiments, M is selected from one or more of lithium, sodium, and potassium.
[0102] In some embodiments, -COOM is any one of -COOLi, -COONa, and -COOK.
[0103] The lithium, sodium or potassium introduced into the fluorine-containing polymer can form ion exchange with the active ions during the charge and discharge process, further increasing the mobility of the active ions, reducing the DC internal resistance of the battery, and improving the kinetic performance of the battery.
[0104] In some embodiments, the molar content of the structural unit derived from the monomer represented by Formula I is 60% to 80%, based on the total molar number of all structural units in the fluorine-containing polymer.
[0105] In some embodiments, the molar content of the structural unit derived from the monomer represented by Formula I can be selected as any value of 60%, 70%, 80%, or a range consisting of any two values thereof, based on the total molar number of all structural units in the fluorinated polymer.
[0106] By controlling the molar content of the structural unit derived from the monomer represented by Formula I within a suitable range, the viscosity of the conductive paste, the cohesive force of the pole piece, and the rebound rate of the pole piece after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0107] In some embodiments, the molar content of the structural unit derived from the monomer shown in formula II is 20%-40%, based on the total moles of all structural units in the fluoropolymer. In some embodiments, the molar content of the structural unit derived from the monomer shown in formula II can be selected as any value of 20%, 30%, 40%, or a range consisting of any two values thereof, based on the total moles of all structural units in the fluoropolymer.
[0108] By controlling the molar content of the structural unit derived from the monomer represented by Formula II within a suitable range, the viscosity of the conductive paste, the cohesion of the pole piece and the rebound rate of the pole piece after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0109] In some embodiments, the weight average molecular weight of the fluorine-containing polymer is 80,000 to 120,000. In some embodiments, the weight average molecular weight of the fluorine-containing polymer can be selected from any value of 80,000, 90,000, 100,000, 110,000, 120,000, or a range consisting of any two values thereof.
[0110] As used herein, the term "weight average molecular weight" refers to the sum of the products of the weight fractions of molecules with different molecular weights in a polymer and their corresponding molecular weights.
[0111] In the present application, the weight average molecular weight of the polymer can be tested by methods known in the art, such as gel chromatography, such as using a Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141) for testing. In some embodiments, the test method is to use a polystyrene solution sample with a mass fraction of 3.0% as a reference, and select a matching chromatographic column (oily: Styragel HT5DMF7.8×300mm+Styragel HT4). Use purified N-methylpyrrolidone (NMP) solvent to prepare a 3.0% fluorine-containing polymer glue, and let the prepared solution stand for one day for use. During the test, first use a syringe to draw tetrahydrofuran, rinse, and repeat several times. Then draw 5 ml of the experimental solution, expel the air in the syringe, and wipe the needle tip dry. Finally, slowly inject the sample solution into the injection port. After the reading stabilizes, obtain the data and read the weight average molecular weight.
[0112] The weight average molecular weight of the fluorinated polymer is controlled within a suitable range so that the slurry has a suitable viscosity, which is beneficial to the subsequent preparation of the negative electrode slurry. At the same time, the fluorinated polymer with a suitable weight average molecular weight is conducive to the formation of a three-dimensional network bonding structure, so that the electrode has good cohesion. The electrode has a low rebound rate after cold pressing for 24 hours. The viscosity of the conductive slurry, the cohesion of the electrode and the rebound rate of the electrode after cold pressing for 24 hours can be taken into account, thereby comprehensively improving the processing performance and use performance of the conductive slurry.
[0113] In one embodiment of the present application, a method for preparing a fluorine-containing polymer is provided, comprising the following steps:
[0114] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0115]
[0116] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, wherein R4, R5, R6 and R7 contain at least two -COOH groups,
[0117] Optionally, the polymerization product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least a portion of -COOH in the polymerization product into -COOM, where M comprises NH4 or an alkali metal.
[0118] In some embodiments, the method for preparing a fluoropolymer comprises the following steps:
[0119] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0120]
[0121] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, wherein R4, R5, R6 and R7 contain at least two -COOH groups.
[0122] In some embodiments, the method for preparing a fluoropolymer comprises the following steps:
[0123] Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product,
[0124]
[0125] wherein R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, wherein R4, R5, R6 and R7 contain at least two -COOH groups,
[0126] The polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least a portion of -COOH in the polymer product into -COOM, wherein M comprises NH4 or an alkali metal.
[0127] In some embodiments, the neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and aqueous ammonia.
[0128] Compared with traditional dispersants, the fluorine-containing polymer prepared by this method can improve the dispersibility of the conductive slurry, alleviate the gelation of the conductive slurry during storage, improve the anti-gelling and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and improve the dynamic performance of the battery. Under the premise, the fluorine-containing polymer can also improve the cohesion of the electrode, reduce the irreversible expansion of the electrode during the manufacturing process, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode.
[0129] In some embodiments, M comprises one or more of lithium, sodium, and potassium.
[0130] In some embodiments, R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
[0131] In some embodiments, the molar content of the monomer represented by formula I is 60%-80%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0132] In some embodiments, the molar content of the monomer represented by formula II is 20%-40%, based on the total moles of the monomer represented by formula I and the monomer represented by formula II.
[0133] In some embodiments, the polymerization reaction specifically comprises:
[0134] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0135] Second stage polymerization: after a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization;
[0136] Optionally, after the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0137] In some embodiments, the polymerization reaction specifically comprises:
[0138] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0139] Second stage polymerization: After a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization.
[0140] In some embodiments, the polymerization reaction specifically comprises:
[0141] First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure;
[0142] Second stage polymerization: after a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization;
[0143] After the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
[0144] The method provided in the present application forms a fluorine-containing segment by first continuously feeding the monomer shown in formula I, so that the fluorine-containing polymer has high thermal stability; and then the monomer shown in formula II is introduced to reduce the contact between the fluorine-containing segment and the external environment, effectively alleviating the gel phenomenon caused by the fluorine element. The fluorine-containing polymer prepared by this method can effectively improve the stability of the conductive slurry, improve the dispersibility of the slurry, improve the cohesion of the pole piece, reduce the pole piece rebound rate after cold pressing for 24 hours, reduce the diaphragm resistance of the pole piece and the DC internal resistance of the battery, and improve the dynamic performance of the battery. In addition, when the monomer shown in formula II is fed into the reaction vessel for the second stage of polymerization, the monomer shown in formula I is continuously fed into the reaction vessel, which helps to improve the compatibility of the segment generated by the first stage of polymerization and the segment generated by the second stage of polymerization, and improve the stability of the fluorine-containing polymer.
[0145] In some embodiments, the mass of the monomer of formula I introduced in the first stage polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
[0146] In some embodiments, the mass percentage of the initiator is 0.5%-1.5%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.
[0147] In some embodiments, the mass percentage of the emulsifier is 0.1%-0.5%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.
[0148] In some embodiments, the mass percentage of the aqueous medium provided in the polymerization reaction is 400%%-600%, based on the total mass of the monomer represented by Formula I and the monomer represented by Formula II.
[0149] In some embodiments, the reaction pressure of the polymerization reaction is 7 MPa-9 MPa, and the reaction temperature of the polymerization reaction is 80° C.-120° C.
[0150] In some embodiments, the initiator is one or both of N,N-dimethylbenzylamine and N-methylamphetamine.
[0151] In some embodiments, the emulsifier is at least one of alkali metal perfluorooctanoate, polyoxyethylene-4-phenol ether ammonium sulfate, and nonylphenol polyoxyethylene ether ammonium sulfate.
[0152] In one embodiment of the present application, there is provided an application of the fluorine-containing polymer in any embodiment in a secondary battery. Optionally, the secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
[0153] [Conductive paste]
[0154] In one embodiment of the present application, a conductive paste is provided, comprising a conductive agent, an aqueous medium, and the fluorine-containing polymer described in any embodiment.
[0155] Compared with the prior art of directly adding a conductive agent during the preparation of the negative electrode slurry, the conductive slurry provided by the present application can improve the dispersibility of the conductive agent in the negative electrode slurry, improve the conductive effect of the conductive agent in the pole piece, and then effectively reduce the content of the conductive agent in the pole piece, which is conducive to further increasing the load of the pole piece and improving the battery power performance. Moreover, the fluorinated polymer in the conductive slurry can play the role of a binder and a dispersant at the same time. On the premise of improving the dispersibility of the conductive slurry, improving the dispersibility of the conductive agent in the pole piece, and reducing the DC impedance of the battery, it can also improve the cohesion of the pole piece, reduce the rebound rate after cold pressing, and improve the quality of the pole piece.
[0156] In some embodiments, the aqueous medium comprises deionized water.
[0157] In some embodiments, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0158] In some embodiments, the conductive agent includes carbon nanotubes.
[0159] The one-dimensional linear carbon nanotubes form a long-range conductive network in the electrode. This conductive network can connect the active material particles together, keep the particles in electrical contact, and give the battery a small DC impedance. At the same time, this conductive network can limit the mutual repulsion between the active material particles after cold pressing, reduce the rebound rate of the electrode after cold pressing, and improve the quality of the electrode.
[0160] In some embodiments, the mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste.
[0161] In some embodiments, the mass fraction of the conductive agent may be any value of 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5%, or a range consisting of any two values thereof, based on the total mass of the conductive paste.
[0162] The mass fraction of the conductive agent is controlled within a suitable range. Based on the total mass of the conductive slurry, the slurry has a suitable viscosity, and the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the slurry.
[0163] In some embodiments, the mass fraction of the fluorinated polymer is 0.5%-1.5%, based on the total mass of the conductive paste. In some embodiments, the mass fraction of the fluorinated polymer is any value of 0.5%, 0.75%, 1%, 1.25%, 1.5%, or a range consisting of any two values thereof, based on the total mass of the conductive paste.
[0164] By controlling the mass fraction of the fluorine-containing polymer within a suitable range, the slurry has a suitable viscosity based on the total mass of the conductive slurry, and the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the slurry.
[0165] In any embodiment, the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500 mPa·s-5000 mPa·s.
[0166] In some embodiments, the solid content of the conductive paste may be any value of 1%, 3%, 5%, 6%, 10%, or a range consisting of any two values thereof.
[0167] In some embodiments, the viscosity of the conductive paste may be selected as any value of 500 mPa·s, 600 mPa·s, 700 mPa·s, 800 mPa·s, 900 mPa·s, 1000 mPa·s, 1100 mPa·s, 1200 mPa·s, 1300 mPa·s, 1400 mPa·s, 1500 mPa·s, 2000 mPa·s, 2500 mPa·s, 3000 mPa·s, 3500 mPa·s, 4000 mPa·s, 4500 mPa·s, or 5000 mPa·s, or a range consisting of any two of the values.
[0168] The solid content is 1%-10%, and the viscosity is 500mPa·s-5000mPa·s. It can be directly mixed and stirred with active materials and binders to prepare negative electrode slurry without adding additional additives, which is beneficial to improving production efficiency and reducing production costs.
[0169] [Negative electrode]
[0170] The fifth aspect of the present application provides a negative electrode plate, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry of the fourth aspect.
[0171] As used herein, the term "binder" refers to a chemical compound, polymer or mixture that forms a colloidal solution or colloidal dispersion in a dispersion medium.
[0172] Compared with the negative electrode plates prepared by directly adding conductive agent powder in the prior art, the conductive agent in the negative electrode plates disclosed in the present application exists in the negative electrode plates in the form of conductive slurry deposits. On the one hand, the cohesion of the plates can be improved, the rebound rate of the plates after cold pressing for 24 hours can be reduced, and the quality of the plates can be improved. On the other hand, adding the conductive slurry can improve the dispersion performance of the conductive material, so that the negative electrode plates can have low membrane resistance when the conductive agent is added in a low amount, which provides the possibility of further increasing the loading amount of the negative electrode active material in the plates.
[0173] In some embodiments, the compaction density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode plate is cold pressed for 24 hours, the plate rebound rate is not higher than 7.0%.
[0174] In this article, the rebound rate of the negative electrode after cold pressing for 24 hours is a well-known meaning in the art and can be measured using instruments and methods known in the art. As an example, the coated negative electrode is cold pressed to a fixed compaction density (1.5 g / cm 3 ), test the thickness of the negative electrode sheet, recorded as h1; after the cold pressed electrode sheet is left to stand for 24 hours, test the thickness of the negative electrode sheet, recorded as h2,
[0175] The rebound rate of the electrode after cold pressing for 24 hours (%) = (h2-h1) / h1×100%.
[0176] Under the premise of meeting the high compaction density of the negative electrode plate and improving the energy density of the battery, the negative electrode plate of the present application has a low rebound rate after cold pressing for 24 hours, which improves the use quality of the plate, improves the quality of the plate, and is beneficial to the subsequent assembly process of the battery.
[0177] In some embodiments, the compaction density of the pole piece can be selected to be 1.3 g / cm 3 , 1.4g / cm 3 , 1.5g / cm 3 , 1.6g / cm 3 , 1.7g / cm 3 Any value in , or a range of any two values in .
[0178] In some embodiments, the rebound rate of the negative electrode plate after cold pressing for 24 hours can be selected as any one of no higher than 7.0%, no higher than 6.0%, and no higher than 5.0%.
[0179] In some embodiments, the cohesive force of the negative electrode plate is not less than 73 N / m, and can be optionally not less than 80 N / m.
[0180] In this article, the cohesion of the negative electrode sheet is a well-known meaning in the art and can be measured using instruments and methods well-known in the art. As an example, a double-sided tape is used to stick on a steel plate, and the negative electrode sheet is cut into a strip with a length of 20 cm and a width of 20 mm and stuck on the double-sided tape. The single-sided adhesive tape (width × length = 20 mm × 80 mm) for testing the cohesion of the negative electrode sheet is centered and stuck to the strip and covers the strip. A white paper strip with a width × length = 20 mm × 60 mm is cut and inserted between the steel plate and the single-sided adhesive tape, with an overlap length of about 15 mm. The strip is rolled back and forth on the strip with a roller 4 times, and the white paper is clamped on the tensile machine fixture. The tensile machine test is turned on to separate the single-sided adhesive tape that sticks to the negative electrode film layer of the strip from the strip. The test is completed to obtain the cohesion value.
[0181] In some embodiments, based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the film resistance of the negative electrode film layer is not higher than 0.15Ω.
[0182] In some embodiments, based on the total mass of the negative electrode film layer, the mass content of the conductive agent can be selected as any value of 0.2%, 0.5%, 1%, 1.5%, 2% or a range consisting of any two values thereof.
[0183] In some embodiments, the sheet resistance of the negative electrode film layer may be selected to be no higher than any one of 0.15Ω, 0.1Ω, and 0.05Ω.
[0184] In this article, the film resistance of the negative electrode film layer has a well-known meaning in the art and can be measured using instruments and methods well-known in the art. As an example, the dried electrode is cut at the left, middle and right of the electrode into small discs with a diameter of 10 mm. Turn on the power of the Yuanneng Technology electrode resistor meter, place it in the appropriate position of the "probe" of the electrode resistor meter, click the "Start" button, and wait for the reading to stabilize before reading. Each small disc is tested at two positions, and finally the average of the six measurements is calculated, which is the film resistance of the electrode.
[0185] As an example, the negative electrode current collector has two surfaces opposite to each other in its thickness direction, and the negative electrode film layer is disposed on any one or both of the two opposite surfaces of the negative electrode current collector.
[0186] In some embodiments, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0187] In some embodiments, the negative electrode active material may adopt the negative electrode active material for the battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0188] In some embodiments, the negative electrode film layer may further include a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0189] In some embodiments, the negative electrode film layer may further include a conductive agent, which may be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0190] In some embodiments, the negative electrode film layer may optionally include other additives, such as a thickener (eg, sodium carboxymethyl cellulose (CMC-Na)).
[0191] In some embodiments, the negative electrode sheet can be prepared in the following manner: the above-mentioned components for preparing the negative electrode sheet, such as the fluorine-containing polymer, the conductive agent, and the deionized water are first stirred to prepare a conductive slurry, and the negative electrode active material, the binder, the conductive slurry and any other components are dispersed in the deionized water to form a negative electrode slurry; the negative electrode slurry is coated on the negative electrode collector, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0192] [Positive electrode]
[0193] The positive electrode sheet includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0194] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0195] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0196] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM 333 )、LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM 523 )、LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM 211 )、LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM 622 )、LiNi 0.8 Co 0.1 Mn0.1 O2 (also referred to as NCM 811 ), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co 0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0197] In some embodiments, the positive electrode film layer may further optionally include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0198] In some embodiments, the positive electrode film layer may further include a conductive agent, which may include, for example, at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0199] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the positive electrode collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0200] [Electrolytes]
[0201] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0202] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0203] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0204] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0205] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0206] [Isolation film]
[0207] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, and any known porous separator with good chemical stability and mechanical stability can be selected.
[0208] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0209] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0210] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0211] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0212] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 1 The secondary battery 5 is a square structure as an example.
[0213] In some embodiments, reference Figure 2, the outer packaging may include a shell 51 and a cover plate 53. Among them, the shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. The number of electrode assemblies 52 contained in the secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.
[0214] In some embodiments, secondary batteries may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0215] Figure 3 4 is an example of a battery module. Figure 3 In the battery module 4, the plurality of secondary batteries 5 may be arranged in sequence along the length direction of the battery module 4. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 5 may be fixed by fasteners.
[0216] Optionally, the battery module 4 may further include a housing having a receiving space, and the plurality of secondary batteries 5 are received in the receiving space.
[0217] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0218] Figure 4 and Figure 5 1 is a battery pack 1 as an example. Figure 5 and Figure 6 The battery pack 1 may include a battery box and a plurality of battery modules 4 disposed in the battery box. The battery box includes an upper box body 2 and a lower box body 3. The upper box body 2 can cover the lower box body 3 and form a closed space for accommodating the battery modules 4. The plurality of battery modules 4 can be arranged in the battery box in any manner.
[0219] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0220] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0221] Figure 6 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0222] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0223] Example
[0224] Hereinafter, the embodiments of the present application will be described. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are indicated in the embodiments, the techniques or conditions described in the literature in this area or the product specifications are used. If the manufacturer is not indicated in the reagents or instruments used, they are all conventional products that can be obtained commercially.
[0225] Example 1
[0226] 1) Preparation of fluorinated polymers
[0227] First stage polymerization: add 30 kg of deionized water (conductivity less than or equal to 2 μs / cm), 15 g of sodium perfluorooctanoate, and 54 g of N,N-dimethylbenzylamine into a 50 L reactor, and close the reactor;
[0228] The reactor was evacuated and filled with nitrogen, and the operation was repeated until the oxygen concentration in the reactor was less than 100 ppm;
[0229] Add vinylidene fluoride monomer into the reactor until the pressure inside the reactor reaches 8.0 MPa;
[0230] The temperature in the kettle was raised to 100°C to start the reaction, and vinylidene fluoride monomer was continuously introduced during the reaction to maintain the reaction pressure in the kettle constant;
[0231] Second stage polymerization: when the mass of the introduced vinylidene fluoride monomer is 1411.1 g, the reaction pressure is maintained at 8.0 MPa and the temperature is 100° C., 1411.1 g of vinylidene fluoride monomer and 3177.8 g of allylmalonic acid monomer are continuously introduced into the reactor, and the reaction is continued for 8 hours;
[0232] When the reaction is completed, the pressure in the autoclave drops to 0.2 MPa, and the unreacted vinylidene fluoride monomer is recovered;
[0233] The reaction product was condensed, washed, and neutralized by adding 1625.58 g of lithium carbonate and stirred for 2 hours; then separated and concentrated to obtain a vinylidene fluoride-allyl lithium malonate copolymer emulsion with a solid content of 25%, wherein the weight average molecular weight of the vinylidene fluoride-allyl lithium propylene copolymer was 100,000.
[0234] 2) Preparation of conductive paste
[0235] 18400 g of deionized water and 800 g of vinylidene fluoride-lithium allyl malonate copolymer emulsion were added into a 35 L stirring tank and stirred at a stirring speed of 800 rpm for 30 min to obtain a prefabricated glue solution;
[0236] Then, 800 g of carbon nanotubes were added to the prefabricated glue solution and stirred at a speed of 800 rpm for 180 min, and cooling water circulation was started to obtain a conductive paste having a solid content of 5%.
[0237] 3) Preparation of negative electrode sheet
[0238] Active material artificial graphite, active material SiO2, binder styrene butadiene rubber (SBR), thickener sodium hydroxymethyl cellulose (CMC), and the above conductive slurry are added into deionized water, mixed evenly and prepared into negative electrode slurry; the negative electrode slurry is evenly coated on the negative electrode current collector copper foil once or multiple times, and the negative electrode sheet is obtained through drying, cold pressing and cutting, wherein in the negative electrode film layer, the weight ratio of the deposits of active material artificial graphite, active material SiO2, binder styrene butadiene rubber (SBR), thickener sodium hydroxymethyl cellulose (CMC) and conductive slurry is 90.8%:5%:3%:1%:0.2%.
[0239] 4) Preparation of positive electrode
[0240] Lithium nickel cobalt manganese (NCM) material, conductive agent carbon black, polyvinylidene fluoride binder, and N-methylpyrrolidone (NMP) are stirred and mixed evenly in a weight ratio of 96.9:2.1:1:21 to obtain a positive electrode slurry with a solid content of 73%. The positive electrode slurry is then evenly coated on the positive electrode collector aluminum foil, and then dried, cold pressed, and cut to obtain a positive electrode sheet.
[0241] 5) Isolation film
[0242] Polypropylene film is used as the isolation film.
[0243] 6) Preparation of electrolyte
[0244] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvents ethylene carbonate (EC) / ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3 / 7, 12.5% LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred evenly to obtain the electrolyte of Example 1.
[0245] 7) Preparation of batteries
[0246] The positive electrode sheet, the separator, and the negative electrode sheet of Example 1 are stacked in order, so that the separator is between the positive and negative electrode sheets to play an isolating role, and then wound to obtain a bare cell, and the bare cell is welded with a pole ear, and the bare cell is placed in an aluminum shell, and baked at 80°C to remove water, and then the electrolyte is injected and sealed to obtain an uncharged battery. The uncharged battery is then subjected to the processes of static, hot and cold pressing, formation, shaping, and capacity testing in sequence to obtain the lithium-ion battery product of Example 1.
[0247] In Examples 2 to 5, the molar ratio of each monomer in the fluorine-containing polymer was adjusted, and other parameters were kept consistent with those in Example 1. The specific parameters are shown in Table 1.
[0248] In Examples 6 to 9, the experimental parameters of the preparation method of the fluorine-containing polymer are adjusted so that the fluorine-containing polymer has different weight average molecular weights. Other parameters are consistent with those in Example 1. The specific parameters are shown in Tables 1 and 2.
[0249] Specifically, the preparation method of the fluorine-containing polymer with a weight average molecular weight of 60,000 in Example 6 is basically the same as the steps in Example 1, except that the amount of N, N-dimethylbenzylamine added is adjusted to 59.4 g and the reaction temperature is adjusted to 105°C.
[0250] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 80,000 in Example 7 is basically the same as the steps in Example 1, except that the amount of N, N-dimethylbenzylamine added is adjusted to 56.7 g and the reaction temperature is adjusted to 105°C.
[0251] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 120,000 in Example 8 is basically the same as the steps in Example 1, except that the reaction temperature is adjusted to 95° C. and the amount of N,N-dimethylbenzylamine added is adjusted to 51.3 g.
[0252] The preparation method of the fluorine-containing polymer with a weight average molecular weight of 150,000 in Example 9 is basically the same as the steps in Example 1, except that the reaction temperature is adjusted to 95° C. and the amount of N,N-dimethylbenzylamine added is adjusted to 48.6 g.
[0253] In Examples 10 to 13, the mass fraction of the fluorine-containing polymer in the conductive paste was adjusted, and other parameters were kept consistent with those in Example 1. The specific parameters are shown in Table 1.
[0254] In Examples 14 to 17, the mass fraction of the conductive agent in the conductive primer slurry was adjusted, and other parameters remained the same as in Example 1. The specific parameters are shown in Table 1.
[0255] In Example 18, the allylmalonic acid monomer is replaced by 2-pentenedioic acid monomer, and other parameters are the same as in Example 1. For specific parameters, see Table 1.
[0256] In Example 19, 1411.1 g of vinylidene fluoride monomer in the first stage polymerization and 1411.1 g in the second stage polymerization were replaced by 960.5 g of vinylidene fluoride and 815.3 g of chlorotrifluoroethylene monomer, respectively. Other parameters were the same as in Example 1. For specific parameters, see Table 1.
[0257] In Example 20, lithium carbonate was not added for neutralization after the polymerization was completed, and other parameters were the same as in Example 1. For specific parameters, see Table 1.
[0258] In Comparative Example 1, the fluorine-containing polymer in the conductive paste is replaced with a dispersant polyvinyl pyrrolidone (PVP), and other parameters are the same as those in Example 1. For specific parameters, see Table 1.
[0259] In Comparative Example 2, polyvinylidene fluoride emulsion is used as the fluorine-containing polymer, and other parameters are the same as those in Example 1. For specific parameters, see Table 1.
[0260] In Comparative Example 3, polyallyl lithium malonate emulsion is used as the fluorine-containing polymer, and other parameters are the same as those in Example 1. For specific parameters, see Table 1.
[0261] In Comparative Example 4, the allylmalonic acid monomer is replaced with 4-pentenoic acid monomer, and other parameters are the same as those in Example 1. For specific parameters, see Table 1.
[0262] In Comparative Example 5, conductive carbon black is used instead of conductive paste to directly prepare the negative electrode plate. Other parameters are the same as those in Example 1. For specific parameters, see Table 1.
[0263] In Comparative Example 6, the mass content of the conductive carbon black was adjusted to 2.0%, based on the total mass of the negative electrode film layer. Other parameters were substantially the same as those in Comparative Example 5. For specific parameters, see Table 1.
[0264] 2. Test Method
[0265] 1. Characterization of Fluorinated Polymers
[0266] (1) Measurement of weight average molecular weight of fluorinated polymer
[0267] A Waters 2695 Isocratic HPLC gel chromatograph (differential refractive index detector 2141) was used. A polystyrene solution sample with a mass fraction of 3.0% was used as a reference, and a matching chromatographic column was selected (oily: Styragel HT5 DMF 7.8×300 mm + Styragel HT4). A 3.0% fluorine-containing polymer solution was prepared with purified N-methylpyrrolidone (NMP) solvent, and the prepared solution was allowed to stand for one day for use. During the test, tetrahydrofuran was first drawn with a syringe and rinsed, and repeated several times. Then 5 ml of the experimental solution was drawn, the air in the syringe was expelled, and the needle tip was wiped dry. Finally, the sample solution was slowly injected into the injection port. After the indication stabilized, the data was obtained and the weight-average molecular weight was read.
[0268] 2. Property test of conductive paste
[0269] (1) Viscosity test of conductive paste
[0270] Use a rotating viscometer to measure the viscosity of the primer slurry. Select a suitable rotor, fix the viscometer rotor, place the primer slurry under the viscometer rotor, and the slurry just submerges the scale line of the rotor. Instrument model: Shanghai Fangrui NDJ-5S, rotor is 62#, the speed is 30 rpm, and the viscosity range of the slurry can be measured from 0 to 1000 mPa·s; rotor is 63#, the speed is 30 rpm, and the viscosity range of the slurry can be measured from 0 to 2000 mPa·s); rotor is 63#, the speed is 12 rpm, and the viscosity range of the slurry can be measured from 2000 to 10000 mPa·s), test temperature: 25℃, test time is 5 minutes, and read the data after the display is stable.
[0271] (2) Filtration performance test of conductive slurry
[0272] Take a 500ml beaker and place it at the lower end of the 200-mesh filter bracket, take 500ml of conductive slurry, place it in the filter and filter, record the time when the volume of the slurry in the beaker reaches 300ml, this time is used to judge the filtration performance of the slurry. If the filtration time is less than 120s, it indicates that the filtration performance of the slurry is good, which is recorded as "Y"; if the slurry cannot pass through the filter, it indicates that the filtration performance of the slurry is poor, which is judged as "N".
[0273] (3) Solid content of conductive paste and the difference in solid content of the upper and lower layers after standing for 24 hours
[0274] Take the copper foil and weigh it in the weight loss rate measuring instrument, record it as M0, and reset it to zero;
[0275] Take a small amount of conductive paste and apply it on the copper foil, then put it into the moisture meter and weigh it, which is recorded as M1;
[0276] Close the device and start drying;
[0277] After the test, record the weighing data as M2, and calculate the solid content, which is (M2-M0) / (M1-M0);
[0278] The solid content of the upper and lower conductive pastes was measured in the same way after standing for 24 hours, and the solid content of the lower conductive paste minus the solid content of the upper conductive paste was taken as the difference in the upper / lower solid content after the conductive paste was allowed to stand for 24 hours.
[0279] (4) Gel state test of conductive paste after 60 days of standing
[0280] Use a steel ruler to pick up the slurry in the beaker and judge whether the slurry is gelled according to the flow state of the slurry. If the slurry does not gel, record it as "No", if the slurry has gel, record it as "Yes";
[0281] Gel: The slurry clumps or does not flow naturally and continuously.
[0282] No gel: The slurry flows naturally and continuously, and the slurry flows on the surface of the steel ruler without lumps.
[0283] 3. Pole performance test
[0284] (1) Cohesion of the electrode
[0285] Use double-sided tape to stick on the steel plate, cut the negative electrode sheet into a strip with a length of 20 cm and a width of 20 mm and stick it on the double-sided tape, stick the single-sided tape (width × length = 20 mm × 80 mm) for testing the cohesion of the negative electrode sheet in the center and cover the strip, cut a white paper strip with a width × length = 20 mm × 60 mm and insert it between the steel plate and the single-sided tape, with an overlapping length of about 15 mm, roll the strip back and forth on the strip with a roller 4 times, clamp the white paper on the tensile testing machine fixture, start the tensile testing machine test, so that the single-sided tape sticking to the negative electrode film layer of the strip is separated from the strip, and the cohesion value is obtained after the test is completed.
[0286] (2) Pole rebound rate after 24 hours of cold pressing
[0287] The coated negative electrode sheet is cold pressed to a fixed compaction density (1.65g / cm 3), test the thickness of the negative electrode sheet, recorded as h1; after the cold pressed electrode sheet is left to stand for 24 hours, test the thickness of the negative electrode sheet, recorded as h2,
[0288] The rebound rate of the electrode after cold pressing for 24 hours (%) = (h2-h1) / h1×100%.
[0289] (3) Diaphragm resistance of the electrode
[0290] Cut the dried pole piece at the left, middle and right of the pole piece into small discs with a diameter of 10mm. Turn on the power of Yuanneng Technology's pole piece resistor meter, place it in the appropriate position of the "probe" of the pole piece resistor meter, click the "start" button, wait for the reading to stabilize, and then read it. Test two positions of each small disc, and finally calculate the average value of six measurements, which is the film resistance of the pole piece.
[0291] 4. Battery performance test
[0292] (1) Battery DC impedance test
[0293] At 25°C, the secondary battery was charged to 4.2V at a constant current rate of 1 / 3C, and then charged to a current of 0.05C at a constant voltage of 4.2V, and left for 5 minutes. Then, it was discharged at a rate of 1 / 3C for 90 minutes, the electrode assembly was adjusted to 50% SOC, and left for 60 minutes, and then discharged at a rate of 4C for 30S, and the 50% SOC discharge DCR was obtained according to the test data.
[0294] III. Analysis of test results of various embodiments and comparative examples
[0295] According to the above method, the fluorine-containing polymer, conductive paste, negative electrode plate and secondary battery of each embodiment and comparative example were prepared respectively, and various parameters were measured. The results are shown in Tables 1 and 2 below.
[0296] Table 1 Preparation parameters and results of fluorinated polymers of Example 1 and Comparative Example 1
[0297]
[0298]
[0299] Table 2 Preparation parameters and test results of Example 2 and Comparative Example 1
[0300]
[0301]
[0302] As can be seen from Table 1 and Table 2, the fluorine-containing polymers of Examples 1 to 20 include structural units derived from vinylidene fluoride or chlorotrifluoroethylene, and further include structural units derived from allyl dilithium, allyl diacid or lithium 2-pentenedioate.
[0303] From the comparison of Examples 1-9 and Examples 18-20 with Comparative Example 1, it can be seen that compared with the traditional polyvinyl pyrrolidone dispersant, the fluorine-containing polymer disclosed in the present application can improve the cohesive force of the electrode, reduce the rebound rate of the electrode after cold pressing for 24 hours, and improve the quality of the electrode. At the same time, it can also significantly alleviate the gelation of the conductive slurry during storage, improve the anti-gelation and storage properties of the conductive slurry, reduce the diaphragm resistance of the electrode, reduce the DC internal resistance of the battery, and thus improve the dynamic performance of the battery.
[0304] From the comparison of Examples 1-9, Examples 18-20 and Comparative Example 2, it can be seen that compared with polyvinylidene fluoride, the fluorine-containing polymer provided in the present application can reduce the viscosity of the conductive paste, improve the filterability of the conductive paste, make the conductive paste less likely to gel during storage, and improve the anti-gel property and storage property of the conductive paste. Due to the improvement of the dispersion performance of the conductive paste, the DC impedance of the battery is further reduced.
[0305] From the comparison of Examples 1-5 and Example 19 with Comparative Example 3, it can be seen that compared with polyallyl lithium malonate, the vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-trifluorochloroethylene-allyl lithium malonate copolymer, and vinylidene fluoride-allyl malonic acid copolymer disclosed in the present application can improve the cohesion of the pole piece, reduce the rebound rate of the pole piece after cold pressing for 24 hours, and improve the quality of the pole piece. At the same time, it can also improve the anti-sedimentation property of the conductive paste, improve the adhesion of the pole piece, and reduce the DC internal resistance of the battery. From the comparison of Examples 1-5 and Comparative Example 4, it can be seen that the vinylidene fluoride-allyl lithium propylene copolymer disclosed in the present application can improve the cohesion of the pole piece, reduce the rebound rate of the pole piece after cold pressing for 24 hours, and improve the quality of the pole piece. At the same time, it can also reduce the viscosity of the conductive paste, improve the filterability of the conductive paste, make the conductive paste less likely to gel during storage, and improve the anti-gel and storage properties of the conductive paste. Due to the improvement of the dispersion performance of the conductive slurry, the DC impedance of the battery is further reduced.
[0306] From the comparison between Example 1 and Example 20, it can be seen that compared with the structural unit derived from allylmalonic acid, the fluorine-containing polymer containing lithium 2-allyl propylene can reduce the DC internal resistance of the battery and improve the dynamic performance of the battery.
[0307] From the comparison between Examples 1-3 and 4-5, it can be seen that the molar content of the structural units derived from vinylidene fluoride is 60%-80%, which is based on the total molar number of all structural units in the fluorine-containing polymer. It can take into account the viscosity of the conductive paste, the cohesive force of the pole piece and the rebound rate of the pole piece after cold pressing for 24 hours, thereby comprehensively improving the processing performance and use performance of the conductive paste.
[0308] From the comparison between Examples 1-3 and 4-5, it can be seen that the molar content of the structural units derived from allyl dilithium propylene is 20%-40%, which is based on the total molar number of all structural units in the fluorine-containing polymer. It can take into account the viscosity of the conductive paste, the cohesive force of the pole piece and the rebound rate of the pole piece after cold pressing for 24 hours, and comprehensively improve the processing performance and use performance of the conductive paste.
[0309] From the comparison between Examples 1, 7-8 and Examples 6 and 9, it can be seen that the weight average molecular weight of the fluorine-containing polymer is 80,000-120,000, which can take into account the viscosity of the conductive paste, the cohesive force of the electrode and the rebound rate of the electrode after cold pressing for 24 hours, and comprehensively improve the processing performance and use performance of the conductive paste.
[0310] The conductive pastes in Examples 1-20 all include carbon nanotubes, deionized water, and vinylidene fluoride-allyl dilithium propylene copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-chlorotrifluoroethylene-allyl lithium malonate copolymer, and vinylidene fluoride-allyl malonic acid copolymer.
[0311] As can be seen from Examples 1, 10-13, the mass fraction of the fluorine-containing polymer is 0.5%-1.5%, based on the total mass of the conductive paste. The paste has a suitable viscosity, and the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the paste.
[0312] As can be seen from Examples 1, 14-17, the mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste. The paste has a suitable viscosity, and the pole piece has a low rebound rate after cold pressing for 24 hours, which comprehensively improves the processing performance and use performance of the paste.
[0313] It can be seen from Examples 1-20 that the solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500mPa·s-5000mPa·s. The conductive paste prepared from the fluorinated polymer does not require the addition of additional dispersants or thickeners to improve processing performance, which helps to improve production efficiency and optimize the production process.
[0314] The negative electrode sheets in Examples 1-20 all include a negative electrode current collector and a negative electrode film layer disposed on at least one surface of the negative electrode current collector, the negative electrode film layer includes a negative electrode active material, a conductive agent and a binder, and the conductive agent includes a deposit of a conductive slurry.
[0315] From the comparison between Examples 1-20 and Comparative Example 6, it can be seen that compared with the negative electrode plates prepared by directly adding conductive agent powder commonly used in the prior art, the negative electrode plates of the present application contain a conductive agent in the form of a deposit of conductive slurry, which is beneficial to reducing the rebound rate of the plates after cold pressing for 24 hours, improving the cohesion of the plates, and improving the quality of the plates. At the same time, it can also reduce the diaphragm resistance of the plates and the DC internal resistance of the battery, and improve the dynamic performance of the battery.
[0316] Comparison of Examples 1-20 with Comparative Example 7 shows that, compared with the negative electrode sheet prepared by directly adding conductive agent powder commonly used in the prior art, the negative electrode sheet disclosed in the present application includes a conductive agent in the form of a conductive slurry sediment, which can effectively reduce the rebound rate of the sheet after cold pressing for 24 hours and improve the quality of the sheet. At the same time, it can also reduce the content of the conductive agent that needs to be added to the negative electrode sheet, which is conducive to improving the energy density of the battery.
[0317] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A fluorine-containing polymer, characterized in that It comprises at least one structural unit derived from a monomer represented by formula I and at least one structural unit derived from a monomer represented by formula II, Wherein, R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOM, M is selected from hydrogen, NH4 or alkali metal.
2. The fluorinated polymer according to claim 1, characterized in that The M comprises one or more of lithium, sodium and potassium.
3. The fluorine-containing polymer according to claim 1 or 2, characterized in that R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
4. The fluorine-containing polymer according to any one of claims 1 to 3, characterized in that The molar content of the structural unit derived from the monomer represented by formula I is 60% to 80%, based on the total molar number of all structural units in the fluorine-containing polymer.
5. The fluorine-containing polymer according to any one of claims 1 to 4, characterized in that The molar content of the structural unit derived from the monomer represented by formula II is 20% to 40%, based on the total molar number of all structural units in the fluorine-containing polymer.
6. The fluorine-containing polymer according to any one of claims 1 to 5, characterized in that The weight average molecular weight of the fluorine-containing polymer is 80,000-120,000.
7. The fluorine-containing polymer according to any one of claims 1 to 6, characterized in that The monomer represented by formula I comprises one or more of vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, chlorotrifluoroethylene and hexafluoropropylene.
8. The fluorine-containing polymer according to any one of claims 1 to 7, characterized in that The monomer represented by formula II comprises one or more of allylmalonic acid, 2-pentaconedioic acid, lithium 2-pentaconedioate, lithium allylmalonic acid, lithium methylenemalonic acid, lithium vinylmalonic acid, lithium butylmalonic acid, lithium glutaconedioate, lithium maleic acid, trans-glutaconedioate, lithium hexamethylenediamine, lithium heptamethylenediamine, lithium octaconedioate, sodium allylmalonic acid, sodium methylenemalonic acid, sodium vinylmalonic acid, sodium allylmalonic acid, sodium 2-(4-pentene)malonic acid, sodium maleic acid, trans-glutaconedioate, sodium hexamethylenediamine, sodium heptamethylenediamine, sodium octaconedioate, potassium allylmalonic acid, potassium methylenemalonic acid, potassium vinylmalonic acid, and potassium heptamethylenediamine.
9. The fluorine-containing polymer according to any one of claims 1 to 8, characterized in that The fluorine-containing polymer includes one or more of vinylidene fluoride-allyl lithium propylene copolymer, vinylidene fluoride-allyl malonic acid copolymer, vinylidene fluoride-sodium butylmalonate copolymer, vinylidene fluoride-2-pentenedioic acid lithium copolymer, vinylidene fluoride-chlorotrifluoroethylene-allyl lithium malonate copolymer, tetrafluoroethylene-allyl lithium propylene copolymer, and vinylidene fluoride-hexafluoropropylene-allyl lithium propylene copolymer.
10. A method for preparing a fluorine-containing polymer, characterized in that: The following steps are involved: Under polymerizable conditions, at least one monomer represented by formula I and at least one monomer represented by formula II are polymerized to form a polymer product, Wherein, R1, R2, and R3 are each independently selected from hydrogen, fluorine, chlorine, or a C 1-3 Alkyl, R4, R5, R6, R7 are each independently selected from hydrogen or substituted or unsubstituted C 1-15 Alkyl, R4, R5, R6 and R7 contain at least two -COOH groups, Optionally, the polymer product is subjected to a neutralization reaction with a neutralizing agent, wherein the neutralization reaction converts at least a portion of -COOH in the polymer product into -COOM, where M is selected from NH4 or an alkali metal.
11. The preparation method according to claim 10, characterized in that: The M comprises one or more of lithium, sodium and potassium.
12. The preparation method according to claim 10 or 11, characterized in that: R1 is fluorine, and R2 and R3 are each independently selected from hydrogen, fluorine, chlorine or trifluoromethyl.
13. The preparation method according to any one of claims 10 to 12, characterized in that: The molar content of the monomer represented by formula I is 60%-80%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.
14. The preparation method according to any one of claims 10 to 13, characterized in that: The molar content of the monomer represented by formula II is 20%-40%, based on the total molar number of the monomer represented by formula I and the monomer represented by formula II.
15. The preparation method according to any one of claims 10 to 14, characterized in that: The polymerization reaction specifically includes: First stage polymerization: providing an initiator, an emulsifier, at least one monomer represented by formula I and a solvent to carry out first stage polymerization, and continuously feeding the monomer represented by formula I during the first stage polymerization to maintain the initial reaction pressure; Second stage polymerization: after a period of reaction, the monomer represented by formula I and the monomer represented by formula II are introduced into the reaction container for second stage polymerization, and the monomer represented by formula I is continuously introduced in the second stage polymerization; Optionally, after the second stage polymerization reaction is completed, the neutralizing agent is added into the reactor to carry out a neutralization reaction.
16. The preparation method according to claim 15, characterized in that: The mass of the monomer of formula I introduced in the first stage polymerization is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction, and the mass of the monomer of formula I introduced in the second stage polymerization reaction is 30%-70% of the total mass of the monomer of formula I supplied in the polymerization reaction.
17. The preparation method according to any one of claims 10 to 16, characterized in that: The neutralizing agent includes one or more of lithium carbonate, sodium carbonate, potassium carbonate, lithium bicarbonate, sodium bicarbonate, potassium bicarbonate, lithium hydroxide, sodium hydroxide, potassium hydroxide, and ammonia water.
18. Use of the fluorine-containing polymer according to any one of claims 1 to 9 in a secondary battery.
19. A conductive paste, characterized in that: The conductive paste comprises a conductive agent, an aqueous medium and the fluorine-containing polymer according to any one of claims 1 to 9.
20. The conductive paste according to claim 19, characterized in that: The mass fraction of the conductive agent is 1.5%-4.5%, based on the total mass of the conductive paste.
21. The conductive paste according to claim 19 or 20, characterized in that: The mass fraction of the fluorine-containing polymer is 0.5%-1.5%, based on the total mass of the conductive paste.
22. The conductive paste according to any one of claims 19 to 21, characterized in that: The solid content of the conductive paste is 1%-10%, and the viscosity of the conductive paste is 500mPa·s-5000mPa·s.
23. A negative electrode sheet, comprising a negative electrode current collector and a negative electrode film layer arranged on at least one surface of the negative electrode current collector, wherein the negative electrode film layer comprises a negative electrode active material, a conductive agent and a binder, and the conductive agent comprises a deposit of the conductive slurry according to any one of claims 19 to 22.
24. The negative electrode sheet according to claim 23, characterized in that: The compaction density of the negative electrode sheet is 1.5 g / cm 3 -1.8g / cm 3 When the negative electrode plate is cold pressed for 24 hours, the plate rebound rate is not higher than 7.0%.
25. The negative electrode sheet according to claim 23 or 24, characterized in that: The cohesive force of the negative electrode plate is not less than 73 N / m, and can be optionally not less than 80 N / m.
26. The negative electrode sheet according to any one of claims 23 to 25, characterized in that: Based on the total mass of the negative electrode film layer, the mass content of the conductive agent is 0.2%-2%, and the film resistance of the negative electrode film layer is not higher than 0.15Ω.
27. A secondary battery, characterized in that: A negative electrode sheet comprising the negative electrode sheet described in any one of claims 23 to 26.
28. The secondary battery according to claim 27, characterized in that: The secondary battery includes at least one of a lithium ion battery, a sodium ion battery, a magnesium ion battery, and a potassium ion battery.
29. An electrical device, characterized in that: The invention comprises a secondary battery selected from the group consisting of:
Citation Information
Patent Citations
Binder composition for power storage device, slurry for electrode of power storage device, electrode of power storage device, and power storage device