Dispersing agent, preparation method thereof and secondary battery

Through the combined dispersant of polymer anchoring material and panthenol, the problem of poor dispersion of the slurry of the positive electrode material of lithium-ion battery is solved, and the performance and cost-effectiveness of the battery are improved.

CN118930727APending Publication Date: 2024-11-12SHENZHEN DYNANONIC INNOVAZONE NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213802.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing dispersants have poor dispersion in the slurry of the positive electrode material of lithium-ion batteries, resulting in agglomeration, increasing processing difficulty and affecting battery performance.

Method used

The combination of polymer anchoring materials and panthenol is used as a dispersant. Through the steric steric hinder effect of polymer anchoring materials and the polyhydroxyl intermolecular action of panthenol, synergistically reduces slurry viscosity and improves fluidity. , inhibit the aggregation of the conductive agent and the positive electrode active material.

Benefits of technology

It effectively improves the dispersion and fluidity of the slurry of the positive electrode material, reduces the cost of battery production, and improves the capacity and circulation performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930727A_ABST
    Figure CN118930727A_ABST
Patent Text Reader

Abstract

The invention relates to a dispersant and a preparation method thereof, and a secondary battery, the dispersant comprises a functional polymer anchoring material and panthenol, and the mass ratio of the polymer anchoring material to the panthenol is 1: (1-10). According to the invention, the two materials are mixed as a dispersing agent, the conductive agent can be adsorbed by utilizing a functional high-molecular anchoring material, and agglomeration among positive electrode material particles is inhibited by virtue of a steric hindrance effect of a solvation chain of the high-molecular anchoring material; the conductive agent and the positive electrode active material can be further dispersed by utilizing a relatively strong intermolecular acting force formed between hydroxyl in the panthenol and the conductive agent; and the macromolecular anchoring material and the panthenol can achieve a synergistic effect, and steric hindrance of various materials in the slurry is reduced, so that the viscosity of the slurry is reduced, and the flowability of the slurry is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of positive electrode materials, and in particular to a dispersant and a preparation method thereof, and a secondary battery. Background Art

[0002] Compared with other types of batteries, lithium-ion batteries have obvious advantages such as high operating voltage, high energy density, good cycle life, high safety and low environmental pollution, so they are widely used. At the same time, in order to further improve the performance of lithium-ion batteries, the most common technical means is to combine positive electrode active materials such as lithium iron phosphate (LiFePO4) with nanotechnology to reduce the size of positive electrode active materials. However, due to the small particles, large specific surface area and high specific energy of nano-scale materials, nano-scale materials are very easy to spontaneously condense during the pulping process, and flocculation occurs, resulting in uneven distribution. Especially after the pulping is completed and left to stand for a period of time, it is easier to form larger secondary particles. This will not only increase the processing difficulty during the pulping process, thereby affecting the yield of the battery, but also reduce the performance of the prepared pole piece, including capacity, cycle performance and consistency. At the same time, in order to make up for the defect of low conductivity of the positive electrode active material, a carbon material conductive agent with strong conductivity is introduced. The conductive agent is usually also a nano-scale particle. In the liquid medium, the positive electrode active material and the conductive agent, as well as the conductive agents themselves, are very likely to attract each other and agglomerate, thereby making the contact between the conductive agent and the positive electrode active material worse, the electron movement channel incomplete, and the electrochemical performance of the electrode reduced.

[0003] In the prior art, most dispersants are added to the positive electrode material slurry to disperse the particles in the positive electrode material slurry, but the existing dispersants have poor dispersion effects and also increase the viscosity of the slurry and deteriorate the fluidity. Therefore, there is an urgent need for a dispersant that can solve the agglomeration of the positive electrode material slurry and improve the slurry processing performance. Summary of the invention

[0004] The purpose of the present application is to provide a dispersant and a preparation method thereof, and a secondary battery, so as to solve the problem that the existing dispersants have poor dispersibility in the slurry of positive electrode materials.

[0005] To achieve the purpose of this application, this application provides the following technical solutions:

[0006] In a first aspect, the present invention provides a dispersant, comprising a functional polymer anchoring material and panthenol, wherein the mass ratio of the polymer anchoring material to the panthenol is 1:(1-10).

[0007] The advantages of the present invention of using the above two materials mixed as dispersants are: 1) the conductive agent is adsorbed by the polymer anchor material, and the steric hindrance effect of its solvation chain inhibits the agglomeration of particles; 2) the hydroxyl groups in panthenol form a strong intermolecular force with the conductive agent to further disperse the conductive agent and the positive electrode active material; 3) the polymer anchor material and panthenol can play a synergistic role in reducing the steric hindrance of various materials in the slurry, thereby reducing the viscosity of the slurry and improving the fluidity of the slurry; 4) both materials have been industrialized, the raw material cost is low and it is easy to obtain, which can reduce the production cost of the battery.

[0008] In one embodiment, the molecular chain of the polymer anchoring material includes a benzene ring and an azomethine group, and the benzene ring and / or the azomethine group forms a connection combination with the panthenol.

[0009] In one embodiment, the polymer anchoring material is further doped with an anchoring group, and the anchoring group is used to provide steric hindrance.

[0010] In one embodiment, the anchoring group includes one or more of camphorsulfonic acid, p-toluenesulfonic acid and sulfosalicylic acid.

[0011] In one embodiment, the molar ratio of the polymer anchoring material to the anchoring group is 1:(0.03-0.06).

[0012] In one embodiment, the panthenol includes one or more of L-panthenol, D-panthenol and DL-panthenol.

[0013] In one embodiment, the weight average molecular weight of the polymer anchoring material is 10,000 to 16,000.

[0014] In one embodiment, the viscosity of the dispersant is 100 mPa·s to 200 mPa·s.

[0015] In one embodiment, the pH value of the dispersant is 6-9.

[0016] In one embodiment, the density of the dispersant is 1.1 g / cm 3 ~1.15g / cm 3 .

[0017] In a second aspect, the present invention provides a method for preparing a dispersant, comprising: placing a precursor of a polymer anchoring material and an oxidant in a solvent A, and obtaining a functional polymer anchoring material after sufficient reaction; mixing the functional polymer anchoring material and panthenol in a mass ratio to obtain a dispersant, wherein the mass ratio of the polymer anchoring material to the panthenol is 1:(1 to 10).

[0018] In one embodiment, after the functional polymer anchoring material is obtained after sufficient reaction, the method includes: soaking the polymer anchoring material in ammonia water to obtain a mixed solution A, washing the mixed solution A after soaking with deionized water and ethanol until it is neutral, and obtaining a washed polymer anchoring material; mixing the washed polymer anchoring material with an organic aqueous solution having an anchoring group and letting the mixture stand to obtain a mixed solution B, washing the mixed solution B after standing with deionized water and ethanol until it is neutral, and obtaining a polymer anchoring material doped with an anchoring group.

[0019] In a third aspect, the present invention provides a secondary battery, comprising a negative electrode plate, an electrolyte and a positive electrode plate, wherein the positive electrode plate comprises a current collector and a positive electrode material layer disposed on the current collector, wherein the positive electrode material layer comprises the dispersant as described in the first aspect, wherein the viscosity of the positive electrode slurry coating the positive electrode material layer is between 8000 mPa·s and 10000 mPa·s 0.5 h after preparation; and the viscosity of the positive electrode slurry 24 h after preparation is less than or equal to 40000 mPa·s. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the implementation methods of the present application or the technical solutions in the prior art, the drawings required for use in the implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some implementation methods of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0021] Figure 1 is a molecular structure diagram of polyaniline in one embodiment;

[0022] Figure 2 is a molecular structure diagram of panthenol in one embodiment;

[0023] Figure 3 is a molecular structure diagram of doped polyaniline in one embodiment;

[0024] Figure 4 is a molecular structure diagram of an organic sulfonic acid in one embodiment;

[0025] Figure 5 is an infrared spectrum of polyaniline in one embodiment;

[0026] Figure 6 The present invention is a flow chart of a method for preparing a dispersant in one embodiment. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.

[0028] Unless otherwise defined, all technical and scientific terms used in this application have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used in this application and in the specification are only for the purpose of describing specific embodiments and are not intended to limit this application. The term "and / or" used in this application includes any and all combinations of one or more of the related listed items.

[0029] In conjunction with the accompanying drawings, some embodiments of the present application are described in detail below. In the absence of conflict, the following embodiments and features in the embodiments can be combined with each other.

[0030] The present application provides a dispersant, which includes a functional polymer anchoring material and panthenol, wherein the mass ratio of the polymer anchoring material to panthenol is 1:(1-10).

[0031] Specifically, the dispersant provided by the present invention is applied to a battery and can be added to the slurry of the positive electrode material. Among them, the types of batteries include but are not limited to lithium ion batteries, sodium ion batteries or potassium ion batteries. The slurry of the positive electrode material includes positive electrode active materials, positive electrode lithium supplement materials and conductive agents. Of course, in other embodiments, the dispersant can also be added to the negative electrode material.

[0032] Among them, the polymer anchor material is a functional polymer. The polymer anchor material can be adsorbed on the conductive agent, increasing the steric hindrance between the conductive agents to avoid the conductive agents from agglomerating due to attraction. In addition, the steric hindrance effect of the solvation chain of the polymer anchor material can inhibit the agglomeration between the conductive agent and the positive electrode active material, thereby improving the dispersibility of the positive electrode material slurry.

[0033] Furthermore, panthenol is a small molecule organic compound with multiple hydroxyl groups. The structural formula of panthenol is as follows: Figure 2As shown. The chain segments of panthenol are connected with multiple hydroxyl functional groups. The presence of multiple hydroxyl groups can play a role of multiple anchoring, more effectively covering the conductive agent particles and the positive electrode active material particles, and reducing the agglomeration between particles; at the same time, the presence of amide groups further increases its broad spectrum. Since most conductive agents are carbon materials, and carbon materials are combined with multiple functional groups (such as hydroxyl or carboxyl, etc.), the hydroxyl, carbonyl and amino groups on panthenol can form intermolecular forces (hydrogen bonds) with the functional groups on the carbon materials. The existence of electrostatic effects reduces the viscosity of the slurry and avoids the attraction and agglomeration between conductive agents or between conductive agents and positive electrode active materials.

[0034] Therefore, the advantages of the present invention of using the above two materials mixed as dispersants are: 1) the conductive agent is adsorbed by the macromolecular effect of the polymer anchoring material, and the steric hindrance effect of its solvation chain inhibits the agglomeration of particles; 2) the strong intermolecular force between the hydroxyl groups in panthenol and the conductive agent is utilized to further disperse the conductive agent and the positive electrode active material; 3) the polymer anchoring material and panthenol can play a synergistic role in reducing the steric hindrance of various materials in the slurry, thereby reducing the viscosity of the slurry and improving the fluidity of the slurry; 4) both materials have been industrialized, the raw material cost is low and it is easier to obtain, which can reduce the production cost of the battery.

[0035] In a specific embodiment, the mass ratio of the polymer anchoring material to panthenol can be 1: 1, 1: 2, 1: 3, 1: 4, 1: 5, 1: 6, 1: 7, 1: 8, 1: 9, 1: 10. When the mass ratio of the polymer anchoring material to panthenol is within the above range, the two can fully exert their own effects, and can also promote the synergistic effect of the two, thereby improving the dispersing ability of the dispersant and reducing the viscosity of the slurry.

[0036] When the mass ratio of the polymer anchoring material to panthenol is less than the above range, the proportion of the polymer anchoring material is too small, which will lead to a decrease in the binding of the polymer anchoring material to panthenol and a poorer synergistic effect of the two. When the mass ratio of the polymer anchoring material to panthenol is greater than the above range, the proportion of panthenol is too small, which will lead to a decrease in the steric hindrance between the polymer anchoring material and the positive electrode material, thereby reducing the fluidity of the slurry.

[0037] In one embodiment, the polymer anchoring material includes a benzene ring and an azomethine group on its molecular chain, and the benzene ring and / or the azomethine group form a connection combination with panthenol. Optionally, the polymer anchoring material may include polyaniline. Polyaniline is a special high molecular polymer with electrical conductivity. The structural formula of polyaniline is as follows: Figure 1As shown. The polyaniline in the dispersant can cooperate with the conductive agent in the positive electrode material to ensure the electrochemical performance of the positive electrode material. The benzene ring and azomethine on polyaniline have a good affinity for the conductive agent, so that polyaniline can be adsorbed on the conductive agent, increasing the steric hindrance between the conductive agents to avoid the conductive agents from attracting and agglomerating. In addition, the steric hindrance effect of the polyaniline solvation chain can inhibit the agglomeration between the conductive agent and the positive electrode active material, thereby improving the dispersibility of the positive electrode material slurry.

[0038] In addition, the polymer anchoring material is a polymer, and panthenol is a small molecule organic substance. After panthenol is mixed with the polymer anchoring material, the hydroxyl group on the panthenol can also form a hydrogen bond with the benzene ring or amino group on the polymer anchoring material, and the hydrogen bond is used to increase the steric hindrance on the polymer anchoring material chain segment, thereby improving the fluidity of the polymer anchoring material in the dispersant, thereby reducing the viscosity of the dispersant. When the dispersant is added to the slurry of the positive electrode material, the panthenol can further play a role in reducing the viscosity of the slurry, so that in the slurry of the same concentration, the slurry of the positive electrode material provided by the present application has better fluidity.

[0039] In one embodiment, the polyaniline includes intrinsic polyaniline, oxidized polyaniline, reduced polyaniline and doped polyaniline.

[0040] Intrinsic polyaniline refers to pure polyaniline that has not been doped. Polyaniline in this state has good electrochemical reaction reversibility and strong charge storage capacity, and is stable to moisture and air. Therefore, using intrinsic polyaniline as a dispersant can improve the stability of the dispersant, as well as improve the moisture and air stability of the positive electrode material slurry.

[0041] Oxidized polyaniline and reduced polyaniline refer to polyanilines with different oxidation degrees formed by complete or partial oxidation of aniline units during the synthesis process. According to the different oxidation degrees, it can be divided into fully reduced (leucoemeraldine, Figure 1 fully reduced polyaniline), monoquinone (protoemeraldine), diquinone (emeraldine), triquinone (nigraniline) and fully oxidized (pernigraniline, Figure 1 These oxidation states can be converted into each other, and both the fully reduced and fully oxidized forms are insulating states. Only the intermediate state can become a conductor after being doped with proton acid.

[0042] Doped polyaniline is formed by introducing external impurities or additives into polyaniline. During the doping process, the imine nitrogen atoms on the main chain of polyaniline are protonated, forming polar and dipole delocalization into the π bonds of the entire molecular chain, thereby improving its conductivity.

[0043] In one embodiment, please refer to Figure 3 , an anchoring group is doped on the polyaniline. Optionally, the types of the anchoring group are as Figure 4 shown, and the anchoring group can be an organic sulfonic acid, including camphorsulfonic acid ( Figure 4 Formula I), p-toluenesulfonic acid ( Figure 4 Formula II) and sulfosalicylic acid ( Figure 4 Formula III), or one or more of them.

[0044] Specifically, the polymer anchoring material in the dispersant provided by the present invention can be doped polyaniline, mainly doped with organic sulfonic acid. The purpose of doping organic sulfonic acid in the polymer anchoring material is to introduce sulfonic acid groups. The sulfonic acid groups significantly enhance the solubility of the polymer anchoring material molecules through their strongly polar sulfonyl (-SO2-OH) moiety. Since the polymer anchoring material itself may have poor solubility, resulting in low utilization rate of the polymer anchoring material as a dispersant, after introducing the sulfonic acid groups, the solubility of the polymer anchoring material is improved, thereby enhancing the fluidity of the dispersant.

[0045] Figure 5 is the infrared spectrum of polyaniline. Among them, (a) is the infrared spectrum of intrinsic polyaniline, (b) is the infrared spectrum of polyaniline in the intermediate oxidation state (0 < y < 0.25), (c) is the infrared spectrum of polyaniline in the intermediate oxidation state (0.75 < y < 1), and (d) is the infrared spectrum of doped polyaniline. It can be Figure 5 seen that the intrinsic polyaniline has strong absorption peaks at 820 cm -1 , 1163 cm -1 , 1300 cm -1 , 1488 cm -1 and 1588 cm -1 . In (d), two characteristic peaks at 1027 cm -1 and 673 cm -1 can be clearly seen, and these two characteristic peaks are both absorption characteristic peaks of the -SO3- group.

[0046] The present invention uses a polymer anchoring material doped with an anchoring group as one of the materials of the dispersant. The conjugated structure formed by the anchoring group and the polymer anchoring material can promote the dispersion of the conductive agent in the slurry through π-π interaction, so as to solve the problem of agglomeration of the conductive agent with nanoscale particles. Moreover, the anchoring group also promotes the activity of panthenol. The anchoring group and panthenol are placed in the chain segments of the polymer anchoring material, enhancing the steric hindrance effect of the solvated chain of the polymer anchoring material and strengthening the inhibition effect on the particle agglomeration in the positive electrode material slurry.

[0047] In one embodiment, at least part of the anchoring group (organic sulfonic acid) and panthenol are connected by hydrogen bonds. Specifically, since panthenol has multiple hydroxyl functional groups, and the oxygen atom in the hydroxyl group has a large electronegativity, and the sulfonic acid group in the organic sulfonic acid has a low electronegativity hydrogen atom, the hydroxyl group on panthenol and the sulfonic acid group on the organic sulfonic acid can form a hydrogen bond.

[0048] In the present application, the polyaniline and panthenol connected by hydrogen bonds have a high bonding strength, and the two synergistically adsorb the conductive agent, which can inhibit the agglomeration of the conductive agent particles. Compared with the single dispersant in the prior art, the dispersant provided by the present invention has better dispersibility for the positive electrode material under the synergistic effect of the two, and can reduce the slurry viscosity.

[0049] In one embodiment, the molar ratio of the polymer anchoring material to the anchoring group is 1:(0.03-0.06). Optionally, the molar ratio of the polymer anchoring material to the anchoring group can be 1:0.03, 1:0.04, 1:0.05, 1:0.06. When the molar ratio of the polymer anchoring material to the anchoring group is within the above range, the modification effect of the anchoring group on the polymer anchoring material can be ensured, and the modification difficulty of the polymer anchoring material can be reduced.

[0050] In one embodiment, panthenol includes one or more of L-panthenol, D-panthenol and DL-panthenol. Specifically, L-panthenol is levorotatory panthenol, D-panthenol is dextrorotatory panthenol, and DL-panthenol is left-right racemic panthenol.

[0051] In one embodiment, the weight average molecular weight of the polymer anchoring material is 10000 to 16000. Optionally, the weight average molecular weight of the polymer anchoring material may be 10000, 11000, 12000, 13000, 14000, 15000, or 16000. When the molecular weight of the polymer anchoring material is within the above range, it is possible to avoid the poor viscosity stabilization effect caused by a small molecular weight, and to avoid the flocculation of the slurry caused by the excessive steric hindrance effect due to a large molecular weight, resulting in uneven distribution.

[0052] In one embodiment, the viscosity of the dispersant is 100mPa·s to 200mPa·s. Optionally, the viscosity of the dispersant may be 100mPa·s, 110mPa·s, 120mPa·s, 130mPa·s, 140mPa·s, 150mPa·s, 160mPa·s, 170mPa·s, 180mPa·s, 190mPa·s, 200mPa·s. When the viscosity of the dispersant is within the above range, the fluidity of the dispersant can be ensured, the viscosity of the dispersant mixed with the positive electrode slurry can be ensured to be within a suitable range, and the coatability of the positive electrode slurry can be improved.

[0053] In one embodiment, the pH value of the dispersant is 6 to 9. Optionally, the pH value of the dispersant may be 6, 7, 8, or 9. Avoid the dispersant being acidic and affecting the performance of the positive electrode active material.

[0054] In one embodiment, the density of the dispersant is 1.1 g / cm 3 ~1.15g / cm 3 Optionally, the density of the dispersant can be 1.1 g / cm 3 , 1.11g / cm 3 , 1.12g / cm 3 , 1.13g / cm 3 , 1.14g / cm 3 , 1.15g / cm 3 .

[0055] In one embodiment, the present invention also provides a method for preparing a dispersant, please refer to Figure 6 , specifically including the following steps:

[0056] Step S10, placing the precursor of the polymer anchoring material and the oxidant in solvent A, and obtaining a functional polymer anchoring material after sufficient reaction.

[0057] Step S20, mixing a functional polymer anchoring material and panthenol in a mass ratio to obtain a dispersant, wherein the mass ratio of the polymer anchoring material to panthenol is 1:(1-10).

[0058] Specifically, in step S10, a precursor of a polymer anchoring material and an oxidant are placed in a solvent A, and a functional polymer anchoring material is obtained after sufficient reaction, which specifically includes: dissolving a certain amount of a precursor of a polymer anchoring material and an oxidant in a solvent A, stirring evenly and standing at room temperature for a period of time, then washing with deionized water and ethanol to neutrality, and drying to obtain a polymer anchoring material, wherein the precursor of the polymer anchoring material can be aniline.

[0059] Optionally, the oxidant includes one or more of ammonium persulfate, hydrogen peroxide, potassium dichromate, potassium iodate and sodium vanadate.

[0060] Optionally, the molar ratio of the precursor of the polymer anchoring material to the oxidant is 1:(1-5), and can be specifically 1:1, 1:2, 1:3, 1:4, or 1:5.

[0061] Optionally, solvent A can be deionized water or an aqueous solution of a doped acid. The doped acid includes one or more of sulfuric acid, hydrochloric acid and phosphoric acid. The concentration of the doped acid is 0.1 mol / L to 5 mol / L. The standing time is 4 h to 72 h.

[0062] Optionally, in step S20, a functional polymer anchoring material and panthenol are mixed in a mass ratio to obtain a dispersant, specifically comprising: first dissolving a certain mass of the polymer anchoring material in an organic solvent to form a solution, then adding a certain mass of panthenol to dissolve in the solution, and uniformly mixing to obtain the dispersant.

[0063] In one embodiment, the dispersant provided by the present invention includes a polymer anchoring material doped with an anchoring group. Based on step S10 of the above embodiment, after sufficient reaction to obtain a functional polymer anchoring material, the following steps are specifically included:

[0064] Step S11, soaking the polymer anchoring material in ammonia water to obtain a mixed solution A, and washing the mixed solution A after soaking with deionized water and ethanol until it is neutral to obtain a washed polymer anchoring material.

[0065] Step S12, mixing the cleaned polymer anchoring material with an organic aqueous solution having an anchoring group and letting it stand to obtain a mixed solution B, and washing the mixed solution B with deionized water and ethanol until it is neutral to obtain a polymer anchoring material doped with an anchoring group.

[0066] Optionally, the anchoring group includes one or more of camphorsulfonic acid, p-toluenesulfonic acid and sulfosalicylic acid. The concentration of the anchoring group is 0.1 mol / L to 5 mol / L. The standing time is 4 h to 72 h.

[0067] The preparation method of the dispersant provided by the present invention is used for preparing the dispersant of the battery. The dispersant is obtained by mixing a polymer anchoring material and panthenol in a preset ratio. The preparation method is simple, and both materials (especially polyaniline) have been industrialized. The raw material cost is low and easy to obtain, which can reduce the production cost of the battery. The prepared dispersant has the advantages that the benzene ring and amino group in the polymer anchoring material are used to adsorb the conductive agent, and the steric hindrance effect of the solvation chain thereof inhibits the agglomeration between particles; the hydroxyl group in panthenol is used to form a strong intermolecular force with the conductive agent to further disperse the conductive agent and the positive electrode active material; the polymer anchoring material and panthenol can play a synergistic role to reduce the steric hindrance of various materials in the slurry, thereby reducing the viscosity of the slurry and improving the fluidity of the slurry.

[0068] In one embodiment, the present invention also provides a secondary battery, which can be a composition system commonly used in the prior art, for example, including a negative electrode plate, an electrolyte, a separator and a positive electrode plate, the electrolyte can be a solid electrolyte or a liquid electrolyte, and when a liquid electrolyte is selected, the use of a separator can be adaptively selected; the positive electrode plate includes a current collector and a positive electrode material layer arranged on the current collector, and the positive electrode material layer includes the dispersant provided above. The secondary battery includes a positive electrode material and a dispersant as provided in the above embodiment. Specifically, the positive electrode material may include a positive electrode active material and a positive electrode lithium supplement material. Optionally, the positive electrode active material may be a phosphate positive electrode active material and a ternary positive electrode active material, and in a specific embodiment, includes one or more of lithium iron phosphate, lithium cobalt oxide, lithium manganese oxide, lithium manganese iron phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, lithium vanadium phosphate fluorophosphate, lithium titanate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.

[0069] In one embodiment, the mass fraction of the dispersant added to the positive electrode material layer is 0.01% to 0.5%. Optionally, the mass fraction of the dispersant added to the positive electrode material layer can be 0.01%, 0.02%, 0.03%, 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, or 0.5%.

[0070] In one embodiment, the viscosity of the positive electrode slurry coated with the positive electrode material layer is 8000 mPa·s to 10000 mPa·s 0.5 h after preparation; the viscosity of the positive electrode slurry 24 h after preparation is less than or equal to 40000 mPa·s.

[0071] The technical solution of the present invention is described in detail below through specific embodiments.

[0072] Example 1

[0073] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP (N-methylpyrrolidone), wherein the mass ratio of polyaniline to panthenol is 1:5, and the weight average molecular weight of polyaniline is 13,000.

[0074] The preparation method of the dispersant provided in this embodiment is as follows:

[0075] 1) Preparation of polyaniline: Aniline and ammonium persulfate were dissolved in deionized water containing hydrochloric acid, the mass ratio of aniline to ammonium persulfate was 1:2, and the concentration of hydrochloric acid was 2 mol / L; after being stirred evenly, the mixture was allowed to stand at room temperature for 24 h, and then washed with deionized water and ethanol until neutral, and dried to obtain polyaniline.

[0076] 2) Preparation of dispersant: polyaniline is dissolved in NMP, and then panthenol is added to the NMP, and the mixture is stirred thoroughly to obtain a dispersant.

[0077] Example 2

[0078] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:1.

[0079] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.

[0080] Example 3

[0081] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:10.

[0082] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 1.

[0083] Example 4

[0084] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:5, and the weight average molecular weight of polyaniline is 13000. Polyaniline is doped with camphorsulfonic acid, and the molar ratio of polyaniline to camphorsulfonic acid is 1:0.045.

[0085] The preparation method of the dispersant provided in this embodiment is as follows:

[0086] 1) Preparation of polyaniline: Aniline and ammonium persulfate were dissolved in deionized water containing hydrochloric acid, the mass ratio of aniline to ammonium persulfate was 1:2, and the concentration of hydrochloric acid was 2 mol / L; after being stirred evenly, the mixture was allowed to stand at room temperature for 24 h, and then washed with deionized water and ethanol until neutral, and dried to obtain polyaniline.

[0087] 2) Preparation of doped polyaniline: A certain amount of polyaniline was soaked in ammonia water for 30 minutes, washed with deionized water and ethanol until neutral, then mixed evenly with an aqueous solution of camphorsulfonic acid and allowed to stand for 24 hours, and washed with deionized water and ethanol until neutral to obtain camphorsulfonic acid-doped polyaniline.

[0088] 3) Preparation of dispersant: camphorsulfonic acid-doped polyaniline is dissolved in NMP, and then panthenol is added to the NMP, and the mixture is stirred thoroughly to obtain a dispersant.

[0089] Example 5

[0090] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:5, and polyaniline is doped with camphorsulfonic acid, wherein the molar ratio of polyaniline to camphorsulfonic acid is 1:0.03.

[0091] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 4.

[0092] Example 6

[0093] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:5, and polyaniline is doped with camphorsulfonic acid, wherein the molar ratio of polyaniline to camphorsulfonic acid is 1:0.06.

[0094] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 4.

[0095] Example 7

[0096] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP, wherein the mass ratio of polyaniline to panthenol is 1:5, and polyaniline is doped with sulfosalicylic acid.

[0097] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 4.

[0098] Example 8

[0099] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP. The reaction temperature is changed to 60° C., and the weight average molecular weight of the obtained polyaniline is 10,000.

[0100] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 4.

[0101] Example 9

[0102] This embodiment provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP. The reaction temperature is controlled to be 0° C., and the weight average molecular weight of the obtained polyaniline is 16,000.

[0103] The steps for preparing the dispersant provided in this embodiment are the same as those in Example 4.

[0104] Comparative Example 1

[0105] This comparative example provides a dispersant, which includes polyaniline and a solvent, and the solvent is NMP.

[0106] Comparative Example 2

[0107] This comparative example provides a dispersant, which includes panthenol and a solvent, and the solvent is NMP.

[0108] Comparative Example 3

[0109] This comparative example provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP (N-methylpyrrolidone), wherein the mass ratio of polyaniline to panthenol is 2:1, and the weight average molecular weight of polyaniline is 13,000.

[0110] Comparative Example 4

[0111] This comparative example provides a dispersant, which includes polyaniline, panthenol and a solvent, wherein the solvent is NMP (N-methylpyrrolidone), wherein the mass ratio of polyaniline to panthenol is 1:20, and the weight average molecular weight of polyaniline is 13,000.

[0112] The dispersant parameters provided by Examples 1 to 9 and Comparative Examples 1 to 4 are shown in Table 1:

[0113] Table 1 Dispersant parameters provided in Examples and Comparative Examples

[0114]

[0115]

[0116] The dispersants provided in the above-mentioned Examples 1 to 9 and the dispersants provided in Comparative Examples 1 to 4 were respectively prepared into positive electrode slurries according to the following methods:

[0117] The dispersant is added to the positive electrode slurry of the lithium iron phosphate battery and named as Verification Example B1-Verification Example B9, Comparative Verification Example B1-Comparative Verification Example B4. Among them, the positive electrode slurry of the lithium iron phosphate battery is mixed with solid dry material and N-methylpyrrolidone (wherein, the weight of N-methylpyrrolidone is 41.75wt% of the total weight of the positive electrode slurry). Taking the total weight as 100wt%: the solid dry material in the positive electrode slurry includes 96.5wt% of lithium iron phosphate, 1.3wt% of Super P and 2.2wt% of polyvinylidene fluoride. Stir polyvinylidene fluoride and Super P in N-methylpyrrolidone at 400 rpm for 20 minutes, add lithium iron phosphate and stir at 200 rpm for 10 minutes, then add the dispersant and stir at 2000 rpm for 70 minutes to obtain the positive electrode slurry.

[0118] The above-mentioned verification examples B1 to B9 and comparative verification examples B1 to B4 were tested as follows, and the test results in Tables 2 and 3 were obtained:

[0119] Viscosity test: Verification Example B1-Verification Example B9, Comparative Verification Example B1-Comparative Verification Example B4, test the viscosity of the slurry at 0.5h and 24h respectively. Select a suitable rotor, fix the viscometer rotor, place the glue under the viscometer rotor, and the glue just submerges the scale line of the rotor. Instrument model: BROOKFIELD DV2T, rotor: LV-04 (64), speed: 15-30r / min, test temperature: 25℃, test humidity: 20RH%~30RH%, test time is 1min, and read the data after the display is stable. The viscosity reference value of the original positive electrode slurry (without adding dispersant) is (10000±2000)mPa·s.

[0120] Table 2 Slurry viscosity test results of verification example and comparative verification example

[0121]

[0122] The positive electrode slurry solid content test method is as follows: take the positive electrode slurry after homogenization for 0.5 hours and apply it on the aluminum foil, and then dry it to obtain the positive electrode sheet. The calculation formula of the positive electrode slurry solid content W is as follows: W = (m1-m0) / (m2-m0) × 100%, where m0 is the mass of the aluminum foil, m1 is the mass of the positive electrode sheet after drying, and m2 is the mass of the wet positive electrode sheet obtained after the positive electrode slurry is applied to the aluminum foil.

[0123] From the test results of Verification Example B1 and Comparative Verification Example B1 and Comparative Verification Example B2 in Table 2, it can be seen that the dispersant prepared by using the polymer anchoring material and panthenol is added to the positive electrode slurry. After 0.5h and 24h of preparing the slurry, the viscosity of the positive electrode slurry of Verification Example B1 is less than that of Comparative Verification Example B1 and Comparative Verification Example B2, and the solid content of Verification Example B1 is also greater than that of Comparative Verification Example B1 and Comparative Verification Example B2. It shows that the dispersant provided by the present invention can achieve the effect of reducing viscosity and increasing solid content on the basis of dispersing the positive electrode material.

[0124] From the test results of Verification Examples B1 to B3 in Table 2, it can be seen that regulating the mass of the polymer anchoring material and panthenol within an appropriate range has a more obvious effect on reducing the viscosity and strengthening the dispersant. In addition, due to the change in the mass of the polymer anchoring material and panthenol, the viscosity change rate of the slurry 0.5h and 24h after preparation will be different, so the mass ratio of the polymer anchoring material and panthenol can be adjusted to achieve the required slurry viscosity in different time periods.

[0125] It can be seen from the test results of Verification Examples B4 to B6 in Table 2 that the effect of reducing viscosity and strengthening can be further achieved by introducing anchoring groups on the polymer anchoring material. This is because the anchoring groups also promote the activity of panthenol. The anchoring groups and panthenol are placed in the chain segments of the polymer anchoring material, which enhances the steric hindrance effect of the solvation chain of the polymer anchoring material, thereby avoiding particle agglomeration and improving the fluidity of the particles.

[0126] From the test results of Verification Examples B7 to B9 in Table 2, it can be seen that the solution provided by the present invention is also applicable to other anchoring groups and polymer anchoring materials with different molecular weights. In addition, the molecular weight of the polymer anchoring material is also positively correlated with the viscosity of the positive electrode slurry.

[0127] The positive electrode slurry provided in the above Verification Examples B1-B9 and Comparative Verification Examples B1-B4 was coated on the current collector to make a positive electrode sheet, and the positive electrode sheet was assembled into a secondary battery, and the electrochemical performance of the secondary battery was tested. The test results are shown below. In addition, the cycle capacity measurement is recorded from the second cycle after the first charge and discharge, that is, the cycle starts from the second cycle after the first charge and discharge.

[0128] Table 3 Battery performance test results of verification example and comparative verification example

[0129]

[0130] It can be seen from the test results of the verification examples and comparative verification examples in Table 3 that the electrochemical performance of verification examples B1 to B9 in the 0.1C first cycle charge and discharge test is at the same level as that of the comparative verification examples. The battery performance of the verification example is improved compared with the comparative verification example after 1C rate capacity and 400 cycles. It can be seen from the test results of verification example B1, comparative verification example B1 and comparative verification example B2 in Table 3 that, compared with the use of a single-component dispersant (comparative verification example), by mixing the polymer anchoring material and panthenol and adding them to the battery, the battery has a higher retention rate after multiple cycles. It can be seen from the test results of verification examples B1-verification examples B3, comparative verification example B3 and comparative verification example B4 in Table 3 that the mixing ratio of the polymer anchoring material and panthenol needs to be controlled within an appropriate range, so as to not only ensure the first cycle capacity of the battery, but also ensure the stable performance of the capacity retention rate after multiple cycles. Therefore, it is proved that the dispersant provided by the present invention has better performance than the existing dispersants.

[0131] In the description of the embodiments of the present application, it should be noted that the orientation or positional relationship of terms such as "center", "up", "down", "left", "right", "vertical", "horizontal", "inside" and "outside" are based on the orientation or positional relationship described in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application.

[0132] What is disclosed above is only a preferred embodiment of the present application, and it certainly cannot be used to limit the scope of rights of the present application. Ordinary technicians in this field can understand that all or part of the processes of implementing the above embodiment and equivalent changes made according to the claims of the present application are still within the scope covered by the present application.

Claims

1. A dispersant, characterized in that: The dispersant comprises a functional polymer anchoring material and panthenol, and the mass ratio of the polymer anchoring material to the panthenol is 1:(1-10).

2. The dispersant according to claim 1, characterized in that The molecular chain of the polymer anchoring material includes a benzene ring and an azomethine group, and the benzene ring and / or the azomethine group form a connection combination with the panthenol.

3. The dispersant according to claim 1, characterized in that The polymer anchoring material is also doped with anchoring groups, and the anchoring groups are used to provide steric hindrance.

4. The dispersant according to claim 3, characterized in that The anchoring group includes one or more of camphorsulfonic acid, p-toluenesulfonic acid and sulfosalicylic acid.

5. The dispersant according to claim 3, characterized in that The molar ratio of the polymer anchoring material to the anchoring group is 1:(0.03-0.06).

6. The dispersant according to claim 1, characterized in that The weight average molecular weight of the polymer anchoring material is 10,000 to 16,000; and / or The viscosity of the dispersant is 100 mPa·s to 200 mPa·s; and / or the pH value of the dispersant is 6 to 9; and / or the density of the dispersant is 1.1 g / cm 3 ~1.15g / cm 3 .

7. A method for preparing a dispersant, characterized in that: include: The precursor of the polymer anchoring material and the oxidant are placed in solvent A, and after sufficient reaction, a functional polymer anchoring material is obtained; The functional polymer anchoring material and panthenol are mixed in a mass ratio to obtain a dispersant, wherein the mass ratio of the polymer anchoring material to the panthenol is 1:(1-10).

8. The method for preparing a dispersant according to claim 7, characterized in that: The method of obtaining the functional polymer anchoring material after sufficient reaction comprises: The polymer anchoring material is immersed in ammonia water to obtain a mixed solution A, and the mixed solution A after immersion is washed with deionized water and ethanol until it becomes neutral to obtain a washed polymer anchoring material; The cleaned polymer anchoring material is mixed with an organic aqueous solution having an anchoring group and allowed to stand to obtain a mixed solution B. The mixed solution B after standing is washed with deionized water and ethanol until it is neutral to obtain a polymer anchoring material doped with an anchoring group.

9. A secondary battery, comprising a negative electrode plate, an electrolyte and a positive electrode plate, wherein the positive electrode plate comprises a current collector and a positive electrode material layer disposed on the current collector, characterized in that: The positive electrode material layer includes the dispersant according to any one of claims 1 to 6.

10. The secondary battery according to claim 9, characterized in that: in, The viscosity of the positive electrode slurry coating the positive electrode material layer is 8000mPa·s to 10000mPa·s 0.5h after preparation; the viscosity of the positive electrode slurry is less than or equal to 40000mPa·s 24h after preparation.