Modified polysulfide rubber, preparation method and application thereof, and polysulfide sealant containing modified polysulfide rubber

Modification of polysulfide rubber through chain breakage and secondary polymerization methods reduces polysulfide bonds, solving the problem of degradation of polysulfide rubber at high temperatures, achieving good sealing performance in low temperature environments, and is suitable for sealing of high-performance aircraft need.

CN118930752APending Publication Date: 2024-11-12XIAN XIFEI CHENGUANG AVIATION TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410999000.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The performance of existing polysulfide rubbers in high-temperature environments is degraded, making it difficult to meet the sealing requirements of high-performance aircraft. The existing modification methods fail to effectively reduce polysulfide bonds, affecting the sealing performance in low-temperature environments.

Method used

The liquid polysulfide rubber is modified by chain breakage and secondary polymerization to reduce polysulfide bonds. The chain breakage reducing agent and diene end group compound are heated under nitrogen atmosphere, and reacted under ultraviolet light to form a Modified polysulfide rubber.

Benefits of technology

It improves the molecular chain strength of polysulfide rubber, improves sealing performance, meets the sealing requirements of high-performance aircraft at low temperatures, and maintains good sealing performance in the range of -55℃~120℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930752A_ABST
    Figure CN118930752A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of rubber modification and sealants, and relates to a modified polysulfide rubber and a preparation method and application thereof.The preparation method of the modified polysulfide rubber and the polysulfide sealant containing the modified polysulfide rubber comprises the steps that S1, a chain scission reducing agent is added into liquid polysulfide rubber raw rubber, and under the nitrogen atmosphere, stirring and heating chain scission are conducted; s2, further adding a diene-terminated compound and a photoinitiator to form a premix; s3, in a nitrogen atmosphere, the premix is heated and subjected to a synthetic reaction under ultraviolet irradiation, and the modified polysulfide rubber is obtained. The liquid polysulfide rubber raw rubber is modified, polysulfide bonds are reduced, the molecular chain strength of the polysulfide rubber is improved, and the sealing performance is good; the further formed polysulfide sealant has good sealing performance in a low-temperature range, and can meet the sealing requirements of high-performance aircrafts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of rubber modification and sealants, and relates to a modified polysulfide rubber, a preparation method and application thereof, and a polysulfide sealant containing the modified polysulfide rubber. Background Art

[0002] Polysulfide sealant has always been a key sealing material used in aircraft engines, which is determined by its excellent oil resistance, low air permeability and good weather resistance. Polysulfide sealant is an elastic sealing material with good bonding strength formed by chemical crosslinking (vulcanization) of liquid polysulfide rubber with low molecular weight. The structure of liquid polysulfide rubber is [-CH2-CH2-S x -]n, its molecular chain contains other chemical bonds such as thermosensitive polysulfide bonds (—SS—) and acetal bonds (—OCO—); when the polysulfide sealant is in use, the long-term use temperature must be maintained at -55℃~120℃ to ensure the sealing performance of the polysulfide sealant. Because when the long-term use temperature is higher than 120℃, the polysulfide sealant will experience problems such as degradation and aging, which seriously affects the application of this medium-resistant polysulfide sealant in high-temperature fields and is difficult to meet the use requirements of modern high-performance aircraft at high temperatures.

[0003] In the prior art, in order to improve the high temperature resistance of medium-resistant polysulfide sealants, researchers have synthesized a polythioether rubber. Although it has good high temperature resistance (long-term use temperature reaches 160°C, short-term use temperature is 200°C) and strength, the main chain of the polythioether rubber molecule contains only -C-C-, -C-S- and -C-O- groups, which makes the main chain have more repeating units, making it difficult to introduce side groups, and prone to crystallization. This increases the difficulty of controlling the synthetic molecular weight and vulcanization process of the polythioether rubber. Therefore, there are still certain problems when using and constructing in low temperature environments. Therefore, the technology for synthesizing polythioether rubber has not yet been widely used in China.

[0004] Based on the defects of the above-mentioned prior art, effective modification of polysulfide rubber has become another way to improve the properties of polysulfide rubber. At present, the modification of polysulfide rubber mainly includes two mechanisms: physical modification and chemical modification. There are many methods for physical modification, but it is difficult to break through the barriers due to the limitations of the structure of polysulfide rubber itself. Therefore, researchers began to look for chemical modification methods. For example, the Chinese patent document with application number CN201810430313.9 discloses a terminal epoxy polysulfide rubber and its preparation and application. The main process is to react the polysulfide rubber with an alkyl lithium reagent in advance, convert the thiol group in the polysulfide rubber into a sulfur-lithium bond, and obtain a sulfur-lithium polymer; then the sulfur-lithium polymer is capped with an epoxy organic chlorine raw material to obtain a modified terminal epoxy polysulfide rubber; however, this modification method does not convert the polysulfide bonds in the polysulfide rubber.

[0005] In summary, although there are many existing methods for modifying polysulfide rubber, due to the presence of a large number of polysulfide bonds in the liquid polysulfide rubber, the performance of the modified polysulfide rubber is still poor in low temperature environments and cannot meet the operating temperature requirements of polysulfide sealants in high-performance aircraft. Summary of the invention

[0006] Aiming at the technical problem that the existing liquid polysulfide rubber raw rubber has more polysulfide bonds, resulting in poor performance of the modified polysulfide rubber in a low temperature environment, the present invention provides a modified polysulfide rubber and a preparation method and application thereof, and a polysulfide sealant containing the modified polysulfide rubber.

[0007] One of the purposes of the present invention is to modify the liquid polysulfide rubber raw rubber by chain breaking and secondary polymerization to reduce polysulfide bonds, thereby improving the strength of the polysulfide rubber molecular chain and improving the sealing performance.

[0008] The second object of the present invention is to provide a polysulfide sealant containing modified polysulfide rubber, which has good sealing performance in a low temperature range and can meet the sealing requirements of high-performance aircraft.

[0009] In order to achieve the above object, the technical solution adopted by the present invention is:

[0010] A method for preparing modified polysulfide rubber comprises the following steps:

[0011] S1, adding a chain-breaking reducing agent to liquid polysulfide rubber raw rubber, stirring and heating to break the chain under a nitrogen atmosphere to form a low-molecular raw rubber mixture; the mass ratio of the liquid polysulfide rubber raw rubber to the chain-breaking reducing agent is (100-500):1;

[0012] S2, sequentially adding a diene terminal compound and a photoinitiator to the low molecular weight rubber mixture to form a premix; the mass ratio of the low molecular weight rubber mixture to the diene terminal compound is (1-10):1, and the molar ratio of the diene terminal compound to the photoinitiator is (10-20):1;

[0013] S3. In a nitrogen atmosphere, the premix is ​​heated to 50° C. to 60° C., and reacted under ultraviolet light for 30 min to 60 min. The obtained product is washed with water and dried to obtain a modified polysulfide rubber.

[0014] It is further defined that in step S1, the chain breaking reducing agent is sodium hydrosulfide, furfuryl methyl sulfide, dithiothreitol, 2,2'-dithiodiethanol or 2-mercaptoethanol; and the heating temperature is 80°C to 120°C.

[0015] It is further defined that in step S2, the diene terminal compound is diethylene glycol divinyl ether or triethylene glycol divinyl ether.

[0016] It is further defined that in step S2, the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide or 2-isopropylthiophene.

[0017] It is further defined that in step S3, the wavelength of the ultraviolet light is 365nm, the power is greater than 100w, and the irradiation is intermittent.

[0018] The modified polysulfide rubber is prepared by using the modified polysulfide rubber preparation method.

[0019] The use of the modified polysulfide rubber as described in the preparation of polysulfide sealant.

[0020] It is further defined that the modified polysulfide rubber can improve tensile strength and elongation at break at room temperature.

[0021] A polysulfide sealant comprises the following raw materials in parts by weight: 100 parts of component A and 8 to 12 parts of component B.

[0022] The component A is composed of the following raw materials in parts by mass: 30 parts of LP31, 70 parts of modified base rubber, 0.5-0.8 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber; the component B is composed of the following raw materials in parts by mass: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3-5 parts of accelerator, 2-3 parts of stearic acid and 0.5-1 part of epoxy curing agent.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention adds a chain-breaking reducing agent to the original rubber, further performs secondary polymerization after chain breaking, and replaces the original -SS- group with -C-S- and -C-O- groups, thereby greatly reducing polysulfide bonds, thereby improving the strength of the polysulfide rubber molecular chain and having good sealing performance within a low temperature range; the sealant formed by the modified polysulfide rubber can meet the sealing requirements of high-performance aircraft at low temperatures.

[0025] 2. The present invention adopts ultraviolet light irradiation to modify the polysulfide rubber and carries out synthetic modification by photochemical method, which is easy to control and realize industrialization.

[0026] 3. The present invention can complete the modification synthesis of existing polysulfide rubber through a two-step method, with fewer reaction steps and low raw material cost, and is suitable for large-scale production.

[0027] 4. The present invention utilizes modified polysulfide rubber to prepare a polysulfide sealant, which has low density, good sealing performance in a wide range of -55°C to 120°C, good weather resistance, excellent adhesion performance, excellent environmental resistance and fuel resistance, and is mainly used for sealing aircraft structures to ensure the safe flight of aircraft in various environments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 is the gel permeation chromatography (GPC) curve of the modified polysulfide rubber of Example 1;

[0029] Figure 2 is the gel permeation chromatography (GPC) curve of the modified polysulfide rubber of Example 2;

[0030] Figure 3 This is the gel permeation chromatography (GPC) curve of the modified polysulfide rubber in Example 3. DETAILED DESCRIPTION

[0031] The technical solution protected by the present invention is described in detail below with reference to the accompanying drawings. Although the accompanying drawings show specific embodiments of the present invention, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments described herein.

[0032] It should be noted that certain words are used in the specification and claims to refer to specific components. Those skilled in the art should understand that technicians may use different nouns to refer to the same component. This specification and claims do not use the difference in nouns as a way to distinguish components, but use the difference in the functions of the components as the criterion for distinction. For example, "including" or "comprising" mentioned throughout the specification and claims is an open term and should be interpreted as "including but not limited to".

[0033] The present invention provides a method for preparing a modified polysulfide rubber, comprising the following steps:

[0034] S1. Add the chain-breaking reducing agent into the liquid polysulfide rubber raw rubber, stir and heat to break the chain in a nitrogen atmosphere to form a low molecular weight raw rubber mixture.

[0035] In step S1 of the present invention, the chain breaking reducing agent is sodium hydrosulfide, furfuryl methyl sulfide, dithiothreitol, 2,2'-dithiodiethanol or 2-mercaptoethanol. The heating temperature is 80°C to 120°C.

[0036] In step S1 of the present invention, the mass ratio of the liquid polysulfide rubber to the chain scission reducing agent is (100-500): 1. Preferably, the mass ratio of the liquid polysulfide rubber to the chain scission reducing agent can be selected from 100:1, 105:1, 110:1, 115:1 or 120:1.

[0037] S2. Add the diene terminal compound and the photoinitiator to the low molecular weight rubber mixture to form a premix.

[0038] In step S2 of the present invention, the diene terminal compound is diethylene glycol divinyl ether or triethylene glycol divinyl ether.

[0039] In step S2 of the present invention, the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide (TPO) or 2-isopropylthioxanthone (ITX).

[0040] In step S2 of the present invention, the mass ratio of the low molecular weight raw rubber mixture to the diene terminal compound is (1-10):1, and the molar ratio of the diene terminal compound to the photoinitiator is (10-20):1.

[0041] Preferably, the mass ratio of the low molecular weight raw rubber mixture to the diene terminal compound is 1:1, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1.

[0042] Preferably, the molar ratio of the diene terminal compound to the photoinitiator is 10:1, 12:1, 14:1, 15:1, 16:1, 18:1 or 20:1.

[0043] S3. In a nitrogen atmosphere, the premix is ​​heated to 50° C. to 60° C., and a synthesis reaction is carried out under ultraviolet light for 30 min to 60 min. The obtained product is washed with water and dried to obtain a modified polysulfide rubber.

[0044] Preferably, the premix is ​​heated to 50° C., 52° C., 55° C., 58° C. or 60° C.; and the synthesis reaction is carried out for 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min.

[0045] In step S3 of the present invention, the wavelength of the ultraviolet light is 365nm and the power is greater than 100w.

[0046] In step S3 of the present invention, intermittent irradiation is used. Specifically, the ultraviolet lamp is irradiated for 5 minutes, then the ultraviolet lamp is turned off for 5 minutes, and then irradiated again, and this cycle is repeated multiple times until the reaction is completely completed. Intermittent ultraviolet irradiation is used mainly because the synthesis reaction is exothermic, and turning off the ultraviolet light is conducive to heat dissipation, avoiding excessive temperature and affecting the synthesis reaction.

[0047] In the present invention, the ultraviolet light synthesis reaction adopts an ultraviolet light synthesis reactor, preferably, a high-light-transmittance glass reactor is adopted, and ultraviolet light is irradiated from the outside to the high-light-transmittance glass reactor; in addition, the high-light-transmittance glass reactor also has stirring, heating and cooling functions to meet the needs of light synthesis reaction.

[0048] The modified polysulfide rubber prepared by the modified polysulfide rubber preparation method can be used as a raw material for the preparation of polysulfide sealants. When used in polysulfide sealants, the modified polysulfide rubber can improve the tensile strength and the elongation at break at room temperature.

[0049] The present invention also provides a polysulfide sealant, comprising the following raw materials in parts by mass: 100 parts of component A and 8 to 12 parts of component B.

[0050] Specifically, component A is composed of the following raw materials in parts by weight: 30 parts of LP31, 70 parts of modified base rubber, 0.5-0.8 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber obtained above.

[0051] Specifically, component B is composed of the following raw materials in parts by weight: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3-5 parts of accelerator, 2-3 parts of stearic acid and 0.5-1 part of epoxy curing agent.

[0052] The modified sealant has greatly improved tensile strength and elongation at break at room temperature. It is used to seal aircraft structures to ensure the safe flight of aircraft in various environments.

[0053] The technical advantages of the modified polysulfide rubber and polysulfide sealant provided by the present invention are described below through several groups of implementation methods and performance tests.

[0054] It should be noted that, unless otherwise specified, the reagents, drugs, instruments, etc. used in the following examples are all conventional products in the field purchased from the market.

[0055] In the following implementation, the liquid polysulfide rubber raw material can be domestic polysulfide rubber or imported Toray polysulfide rubber. The domestic polysulfide rubber model is JLY121, JLY1225 or JLY155, and the Toray polysulfide rubber model is LP12, LP23, LP31, LP33 or LP980.

[0056] Example 1

[0057] The preparation method of the modified polysulfide rubber provided in this embodiment comprises the following steps:

[0058] S1. Add 500g of Toray polysulfide gum LP31 and 5g of dimercaptoethanol into a three-necked reaction flask to form a mixed solution, stir for 6h under nitrogen protection, and react at a heating temperature of 90°C to form a low molecular gum mixture.

[0059] S2. Add the diene terminal compound and the photoinitiator to the low molecular weight rubber mixture to form a premix. The mass ratio of the low molecular weight rubber mixture to the diene terminal compound is 5:1, and the molar ratio of the diene terminal compound to the photoinitiator is 15:1. The diene terminal compound is triethylene glycol divinyl ether, and the photoinitiator is TPO.

[0060] S3. Then the premix is ​​stirred and transferred to a photosynthesis reactor, heated to 50°C, and irradiated with ultraviolet light for 30 minutes to cause a synthesis reaction. After the reaction is completed, the synthetic product is washed with water and dried to obtain a modified polysulfide rubber.

[0061] In this embodiment, the prepared modified polysulfide rubber is modified and its molecular weight is obtained by gel permeation chromatography.

[0062] from Figure 1 It can be seen that the number average molecular weight of the modified polysulfide rubber prepared in this embodiment is 7042.

[0063] Example 2

[0064] The preparation method of the modified polysulfide rubber provided in this embodiment comprises the following steps:

[0065] S1. Add 500g of domestic polysulfide rubber JLY1225 and 5g of sodium hydrosulfide into a three-necked flask to form a mixed solution, stir for 4h under nitrogen protection, and react at a heating temperature of 100°C to form a low molecular weight rubber mixture.

[0066] S2. Add the diene terminal compound and the photoinitiator to the low molecular weight rubber mixture to form a premix. The mass ratio of the low molecular weight rubber mixture to the diene terminal compound is 5:1, and the molar ratio of the diene terminal compound to the photoinitiator is 15:1. The diene terminal compound is diethylene glycol divinyl ether, and the photoinitiator is TPO.

[0067] S3. Then the premix is ​​stirred and transferred to a photosynthesis reactor, heated to 55°C, and irradiated with ultraviolet light for 30 minutes to cause a synthesis reaction. After the reaction is completed, the synthetic product is washed with water and dried to obtain a modified polysulfide rubber.

[0068] In this embodiment, the prepared modified polysulfide rubber is modified and its molecular weight is obtained by gel permeation chromatography.

[0069] from Figure 2 It can be seen that the number average molecular weight of the modified polysulfide rubber prepared in this embodiment is 4038.

[0070] Example 3

[0071] The preparation method of the modified polysulfide rubber provided in this embodiment comprises the following steps:

[0072] S1. Add 600g of domestic polysulfide rubber JLY155 and 5g of 2,2'-dithiodiethanol into a three-necked flask to form a mixed solution, stir for 4h under nitrogen protection, and react at a heating temperature of 100°C to form a low molecular weight rubber mixture.

[0073] S2. Add the diene terminal compound and the photoinitiator to the low molecular weight rubber mixture to form a premix. The mass ratio of the low molecular weight rubber mixture to the diene terminal compound is 5:1, and the molar ratio of the diene terminal compound to the photoinitiator is 15:1. The diene terminal compound is diethylene glycol divinyl ether, and the photoinitiator is TPO.

[0074] S3. Then the premix is ​​stirred and transferred to a photosynthesis reactor, heated to 60°C, and irradiated with ultraviolet light for 30 minutes to cause a synthesis reaction. After the reaction is completed, the synthetic product is washed with water and dried to obtain a modified polysulfide rubber.

[0075] In this embodiment, the prepared modified polysulfide rubber is modified and its molecular weight is obtained by gel permeation chromatography.

[0076] from Figure 3 It can be seen that the number average molecular weight of the modified polysulfide rubber prepared in this embodiment is 5328.

[0077] Example 4

[0078] This embodiment provides a polysulfide sealant, including the following raw materials in parts by mass: 100 parts of component A and 10 parts of component B.

[0079] In this embodiment, component A is composed of the following raw materials in parts by weight: 30 parts of LP31, 70 parts of modified base rubber, 0.5 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber prepared in Example 1.

[0080] In this embodiment, component B is composed of the following raw materials in parts by weight: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3 parts of accelerator, 2 parts of stearic acid and 1 part of epoxy curing agent.

[0081] Example 5

[0082] This embodiment provides a polysulfide sealant, including the following raw materials in parts by mass: 100 parts of component A and 10 parts of component B.

[0083] In this embodiment, component A is composed of the following raw materials in parts by weight: 30 parts of LP31, 70 parts of modified base rubber, 0.5 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber prepared in Example 2.

[0084] In this embodiment, component B is composed of the following raw materials in parts by weight: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3 parts of accelerator, 2 parts of stearic acid and 1 part of epoxy curing agent.

[0085] Example 6

[0086] This embodiment provides a polysulfide sealant, including the following raw materials in parts by mass: 100 parts of component A and 10 parts of component B.

[0087] In this embodiment, component A is composed of the following raw materials in parts by weight: 30 parts of LP31, 70 parts of modified base rubber, 0.5 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber prepared in Example 3.

[0088] In this embodiment, component B is composed of the following raw materials in parts by weight: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3 parts of accelerator, 2 parts of stearic acid and 1 part of epoxy curing agent.

[0089] In order to verify the performance of the modified polysulfide rubber and sealant of the present invention, the following performance tests were conducted.

[0090] Test 1

[0091] In this test, the three polysulfide sealants prepared in Examples 4 to 6 above were tested for their properties, including base paste viscosity, fluidity, active period, non-stick period, hardness, vulcanization period, density, room temperature tensile strength, and room temperature elongation at break.

[0092] The testing methods for the above performance indicators are in accordance with the GB / T 528-2009 standard method, and the test results are shown in Table 1.

[0093] Table 1 Comparison of performance of different polysulfide sealants

[0094]

[0095]

[0096] From the results in Table 1, it can be seen that the peel strength data of the polysulfide sealant made of the modified polysulfide rubber is much greater than the material requirement of 1.8Mpa, and the sealant has no cracks, powdering, peeling or loss of adhesion. The room temperature tensile strength and room temperature elongation at break are greatly improved, indicating that the prepared sealant has excellent sealing performance and good adhesion performance, and can be used for sealing aircraft structures to ensure the safe flight of aircraft in various environments.

[0097] Test 2

[0098] During the use of sealants, due to the effect of heat, their physical and mechanical properties will be significantly reduced, thus affecting the sealing effect; the heat aging test can be used to understand the degree of performance degradation of sealants in hot air. The test principle is to measure the tensile properties of sealants after accelerated aging under hot air conditions to evaluate the aging performance of sealants.

[0099] The heat-resistant air aging test was carried out according to the standard test method at 150°C to test the tensile properties of the sealant of Example 6. The results are shown in Table 2.

[0100] Table 2 Thermal aging properties of sealants

[0101] Test conditions Tensile strength Ts / MPa Bending strength Eb / % Reference Standards ≥1.2 ≥100 150℃*24h 3.0 315

[0102] It can be seen from Table 2 that the performance test results are all greater than the indicators, with good high temperature resistance and good weather resistance.

[0103] Test 3

[0104] The sealant has good low-temperature performance. When the operating temperature drops to a certain range, the movement of its molecular chain segments gradually slows down. When the ambient temperature drops to the critical temperature of the material, the sealant will lose its softness at room temperature and become glassy. It cannot adapt to the deformation caused by the displacement of the sealing component. The sealant part will become brittle and lose its application value.

[0105] The low temperature flexibility test is to determine the use limit of the material at low temperature. The principle of the low temperature flexibility test is to treat the sealant at low temperature for a certain period of time, and then force it to bend and deform instantly along a certain radius at low temperature to observe the adhesion of the sealant and whether cracks occur.

[0106] The sealant product was subjected to a low-temperature flexibility test at -55°C. No cracks or breaks were found on the sealant surface, and there was no debonding between the sealant and the metal test piece, proving that it has good low-temperature resistance.

[0107] Test 4

[0108] The fuel resistance of the sealant of Example 6 was tested according to the standard test method. The results are shown in Table 3.

[0109] Table 3 Fuel resistance of sealants

[0110] Test conditions Tensile strength Ts / MPa Bending strength Eb / % Reference Standards ≥1.4 ≥150 60℃×14d RP-3 3.2 325

[0111] From the results in Table 3, it can be seen that the polysulfide sealant made of modified polysulfide rubber has excellent fuel resistance, and the test results are all greater than the index requirements, and its fuel resistance is excellent.

[0112] The above tests show that the polysulfide sealant made of modified polysulfide rubber in the present invention has excellent sealing performance, good weather resistance, excellent adhesion performance, environmental protection and non-toxicity, flexibility and plasticity. Compared with conventional aviation sealants, the product has low density, good sealing performance in the range of -55℃ to 120℃, low toxic side effects and environmental pollution, is beneficial to labor protection and environmental protection, has good construction process performance and environmental performance, excellent environmental resistance and fuel resistance, and also has bonding and flame retardant effects.

[0113] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the scope of protection of the invention.

Claims

1. A method for preparing a modified polysulfide rubber, characterized in that: The following steps are involved: S1, adding a chain-breaking reducing agent to liquid polysulfide rubber raw rubber, stirring and heating to break the chain under a nitrogen atmosphere to form a low-molecular raw rubber mixture; the mass ratio of the liquid polysulfide rubber raw rubber to the chain-breaking reducing agent is (100-500):1; S2, sequentially adding a diene terminal compound and a photoinitiator to the low molecular weight rubber mixture to form a premix; the mass ratio of the low molecular weight rubber mixture to the diene terminal compound is (1-10):1, and the molar ratio of the diene terminal compound to the photoinitiator is (10-20):1; S3. In a nitrogen atmosphere, the premix is ​​heated to 50° C. to 60° C., and reacted under ultraviolet light for 30 min to 60 min. The obtained product is washed with water and dried to obtain a modified polysulfide rubber.

2. The method for preparing the modified polysulfide rubber according to claim 1, characterized in that: In the step S1, the chain breaking reducing agent is sodium hydrosulfide, furfuryl methyl sulfide, dithiothreitol, 2,2'-dithiodiethanol or 2-mercaptoethanol; and the heating temperature is 80°C to 120°C.

3. The method for preparing the modified polysulfide rubber according to claim 1, characterized in that: In the step S2, the diene terminal compound is diethylene glycol divinyl ether or triethylene glycol divinyl ether.

4. The method for preparing the modified polysulfide rubber according to claim 1, characterized in that: In the step S2, the photoinitiator is 2,4,6-trimethylbenzoyl-diphenylphosphine oxide or 2-isopropylthiophene.

5. The method for preparing the modified polysulfide rubber according to claim 1, characterized in that: In step S3, the wavelength of the ultraviolet light is 365nm, and the power is greater than 100w; the irradiation is intermittent.

6. Modified polysulfide rubber prepared by the method for preparing modified polysulfide rubber according to claim 1.

7. Use of the modified polysulfide rubber as claimed in claim 6 in the preparation of polysulfide sealant.

8. The use according to claim 7, characterized in that The modified polysulfide rubber can improve the tensile strength and room-temperature breaking elongation of the polysulfide sealant.

9. A polysulfide sealant, characterized in that: The method comprises the following raw materials in parts by weight: 100 parts of component A and 8 to 12 parts of component B; The component A is composed of the following raw materials by weight: 30 parts of LP31, 70 parts of modified base rubber, 0.5-0.8 parts of E44, 1.5 parts of KH590, 0.5 parts of KH560 and 0.3 parts of stearic acid; the modified base rubber is the modified polysulfide rubber according to claim 6; The B component is composed of the following raw materials in parts by weight: 80 parts of manganese dioxide, 60 parts of dibutyl ester, 3-5 parts of accelerator, 2-3 parts of stearic acid and 0.5-1 part of epoxy curing agent.