Water-based polymer dispersing agent as well as preparation method and application thereof

Through the preparation method of aqueous polymer dispersant without organic solvents, the synthesis process is simplified, the performance is improved, the problems of environmental pollution and high production costs in the prior art are solved, and high-quality coating performance is achieved.

CN118930760APending Publication Date: 2024-11-12SHENGHONG (SHANGHAI) NEW MATERIAL TECH CO LTD +1
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411184884.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing water-based coating dispersant synthesis methods require the use of organic solvents, which leads to environmental pollution, high production costs, complex processes and poor performance, affecting the quality of the coating.

Method used

The preparation method of aqueous polymer dispersant without organic solvents is adopted, and the polymerization process is controlled, the process is simplified, and the performance of dispersant is improved by combining polyoxyethylene ether monomers and specific additives.

Benefits of technology

It reduces production costs and environmental pollution risks, simplifies the synthesis process, improves the performance of dispersant, and makes the stability and quality of the coating reach the traditional level, and meets environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005013233640000041
    Figure BDA0005013233640000041
  • Figure BDA0005013233640000101
    Figure BDA0005013233640000101
  • Figure BDA0005013233640000151
    Figure BDA0005013233640000151
Patent Text Reader

Abstract

The invention provides a water-based polymer dispersant as well as a preparation method and application thereof. The preparation raw materials of the water-based polymer dispersant comprise the following components: 10-30 parts of a monomer; 5-25 parts of an auxiliary agent; 50 to 85 parts of a polyoxyethylene ether monomer; 0.2 to 0.6 part of an initiator; 0.75 to 1.6 parts of a chain transfer agent; 50 to 90 parts of deionized water; the auxiliary agent comprises any one or a combination of at least two of dipropylene glycol monomethyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether and dodecanol ester. The preparation raw materials of the water-based polymer dispersant provided by the invention do not contain an organic solvent, solvent removal is not needed in the preparation process, and the water-based polymer dispersant is safe, environment-friendly and simple in process; meanwhile, a macromonomer (polyoxyethylene ether monomer) is adopted to provide a side chain, a specific auxiliary agent is introduced, and the proportion of the auxiliary agent is controlled, so that the problem that the system viscosity is too high in bulk polymerization is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings and relates to an aqueous polymer dispersant and a preparation method and application thereof. Background Art

[0002] Pigments are colored fine particulate substances that are usually insoluble in media such as oil, water, resins and organic solvents. They have good coloring, hiding power and light stability, and are therefore widely used in inks, coatings, printing and dyeing and other industries. Pigments used in coatings usually appear in the form of agglomerates or tiny particles. In order to avoid problems such as coarse particles, flocculation, whitening, reduced gloss and insufficient hiding power during the use of coatings, these particles must be dispersed into a stable dispersion system. In the current low-carbon economy, environmental protection awareness is increasing, and the coatings industry is gradually shifting from traditional solvent-based coatings to environmentally friendly coatings. As a result, water-based coatings have a growing market share in applications such as wood, automobiles, containers and anti-corrosion. However, the surface tension of water is significantly higher than that of solvents, which requires the addition of dispersants to enhance the wetting of the surface of pigment particles to promote their stable dispersion in water.

[0003] At present, there are many methods for synthesizing dispersants, among which solution polymerization is the most common method, which prepares dispersants by polymerization reaction in solvent. Although this method has some advantages, such as relatively mild reaction conditions and easy control of polymerization degree and molecular weight distribution, it is also accompanied by some defects that cannot be ignored, such as the use and recovery of solvents: solution polymerization requires the use of a large amount of organic solvents, which not only increases costs but also may cause environmental pollution. The recovery and reuse of solvents is also a technical challenge, requiring additional equipment and processes, which increases the overall production cost; wide molecular weight distribution: although solution polymerization can control the molecular weight of the polymer to a certain extent, compared with other polymerization methods, such as emulsion polymerization, the molecular weight distribution of the polymer produced is wider, which may affect the performance of the final product; product purity and post-processing: the polymer produced by solution polymerization needs to be separated from the solvent by evaporation or precipitation. These steps may result in low product purity and require further purification, thereby increasing production cost and complexity; energy consumption: the evaporation and recovery process of the solvent usually consumes a lot of energy, especially in industrial-scale production, energy consumption has become an important economic and environmental consideration; safety risks: the use of large amounts of organic solvents may bring the risk of fire and explosion, which requires strict safety measures to prevent, which also increases production costs.

[0004] In order to solve the above problems, some existing technical solutions have proposed new synthesis methods, such as solvent-free synthesis method, microemulsion synthesis method, etc. Although these methods can reduce the use of solvents to a certain extent, their synthesis process is often complicated and requires the use of some special equipment, which increases the difficulty and cost of production. In general, there are still some problems and shortcomings in the existing water-based dispersant synthesis methods. First, most of these methods require the use of organic solvents, which not only increases production costs, but also may cause pollution to the environment. Secondly, the synthesis process of these methods is often complicated and requires the use of some special equipment, which increases the difficulty and cost of production. Finally, the performance of the dispersants synthesized by these methods may not be as good as traditional dispersants, which may affect the quality and performance of the coating.

[0005] CN112898504A discloses a method for preparing a coating dispersant and a coating dispersant. The invention discloses a method for preparing a coating dispersant with high wettability, and the dispersant is a polyether dispersant with polyether as a branch chain. The side chain of the dispersant is composed of a polyether with a molecular weight of 400, and the polyether molecular chain has a good hydrophilic effect, so that the dispersant can have good moisture retention in the slurry, can keep the slurry uniform, and reduce the possibility of slurry bleeding. In addition, the short-chain dispersant molecules have good adsorption, can tightly coat the slurry particles, and have high dispersion performance.

[0006] CN109897443A discloses a method for preparing a coating dispersant. The dispersant is mainly obtained by free radical solution polymerization using acrylic monomers as raw materials. The dispersant of the invention can effectively reduce the surface tension of water-based coatings, enhance the wettability of the dispersant on the pigment surface, improve the binding force with the coating surface groups, and enable the pigment particles to be evenly and stably dispersed in water.

[0007] CN117866158A discloses a novel hyperdispersant and its preparation method and application. The invention uses acrylic monomers as raw materials and obtains a hyperdispersant with long and complex side chains through two solution polymerization reactions. Since the dispersant has multiple anchoring groups and greater steric hindrance, it has better dispersibility and stability. In addition, the dispersant can effectively and stably disperse the pigment in water, and the prepared color paste also has good stability and low viscosity.

[0008] However, the above-mentioned prior arts all adopt solution polymerization to prepare the dispersant, which has the defects of solution polymerization mentioned above.

[0009] Therefore, it is desirable in the art to develop an aqueous dispersant that can be synthesized without using an organic solvent, has a simple preparation method, and has excellent dispersant performance. Summary of the invention

[0010] In view of the deficiencies of the prior art, the purpose of the present invention is to provide an aqueous polymer dispersant and a preparation method and application thereof. The present invention provides a method for synthesizing an aqueous polymer dispersant with excellent performance without using an organic solvent, thereby reducing production costs and reducing pollution to the environment; simplifying the synthesis process of the aqueous polymer dispersant, avoiding the use of special equipment, and reducing production difficulty and cost; improving the performance of the synthesized aqueous polymer dispersant through an improved method, making it comparable to traditional dispersants, thereby improving the quality and performance of the coating. Through these technical improvements, the present invention not only optimizes the bulk polymerization process, but also provides a new way to synthesize high-performance aqueous polymer dispersants, which helps to promote progress in the field of polymer dispersant material production.

[0011] To achieve this object, the present invention adopts the following technical solutions:

[0012] In a first aspect, the present invention provides an aqueous polymer dispersant, wherein the raw materials for preparing the aqueous polymer dispersant include the following components in parts by weight:

[0013]

[0014]

[0015] The auxiliary agent includes any one of dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, and dodecyl alcohol ester, or a combination of at least two of them.

[0016] The aqueous polymer dispersant provided by the present invention does not contain organic solvents in its preparation raw materials, does not need to be solvent removed during the preparation process, is safe and environmentally friendly, and has a simple process; at the same time, by adopting macromolecular monomers (polyoxyethylene ether monomers) to provide side chains, introducing specific additives, and controlling their proportions, the problem of excessively high system viscosity occurring in bulk polymerization is solved.

[0017] In the present invention, the raw materials for preparing the aqueous polymer dispersant are calculated by weight, and the amount of the monomer used can be 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, 26 parts, 28 parts, 30 parts, etc.

[0018] In the present invention, the raw materials for preparing the aqueous polymer dispersant are calculated by weight, and the amount of the auxiliary agent used can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts, 12 parts, 14 parts, 16 parts, 18 parts, 20 parts, 22 parts, 24 parts, or 25 parts.

[0019] In the present invention, the raw materials for preparing the aqueous polymer dispersant are measured in parts by weight, and the amount of the polyoxyethylene ether monomer used can be 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, 68 parts, 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, 84 parts, 85 parts, etc.

[0020] In the present invention, the raw materials for preparing the aqueous polymer dispersant are calculated by weight, and the amount of the initiator used can be 0.2 parts, 0.3 parts, 0.4 parts, 0.5 parts, 0.6 parts, etc.

[0021] In the present invention, the raw materials for preparing the aqueous polymer dispersant are calculated by weight, and the amount of the chain transfer agent used can be 0.75 parts, 0.8 parts, 0.9 parts, 1 parts, 1.1 parts, 1.2 parts, 1.3 parts, 1.4 parts, 1.5 parts, 1.6 parts, etc.

[0022] In the present invention, the raw materials for preparing the aqueous polymer dispersant are measured in parts by weight, and the amount of deionized water used can be 50 parts, 52 parts, 54 parts, 56 parts, 58 parts, 60 parts, 62 parts, 64 parts, 66 parts, 68 parts, 70 parts, 72 parts, 74 parts, 76 parts, 78 parts, 80 parts, 82 parts, 84 parts, 86 parts, 88 parts, 90 parts, etc.

[0023] Preferably, the monomer includes any one of acrylic acid, isooctyl acrylate, methacrylic acid, octadecyl acrylate, isobornyl acrylate, lauryl methacrylate, styrene, n-butyl acrylate, and fumaric acid, or a combination of at least two thereof.

[0024] Preferably, the polyoxyethylene ether monomer includes ethyleneoxypolyoxyethylene ether.

[0025] Preferably, the ethyleneoxy polyoxyethylene ether includes ethyleneoxy polyoxyethylene ether 3000 and / or ethyleneoxy polyoxyethylene ether 600.

[0026] Preferably, the initiator comprises azobisisobutyronitrile.

[0027] Preferably, the chain transfer agent comprises 3-mercaptopropionic acid.

[0028] Preferably, the raw materials for preparing the aqueous polymer dispersant also include an alkali neutralizer.

[0029] Preferably, the alkaline neutralizing agent includes any one of aqueous ammonia, sodium hydroxide solution, triethylamine, or a combination of at least two thereof.

[0030] Preferably, the base neutralizer is used in an amount to adjust the pH value of the aqueous polymer dispersant to neutral.

[0031] Preferably, the solid content of the aqueous polymer dispersant is 20% to 40%, for example, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, etc.

[0032] In a second aspect, the present invention provides a method for preparing the aqueous polymer dispersant as described in the first aspect, the preparation method comprising the following steps:

[0033] (1) adding the formulated amount of polyoxyethylene ether monomer and auxiliary agent into a reactor, heating it, and then adding an initiator;

[0034] (2) Mixing the monomer and the chain transfer agent, adding the obtained mixed solution to the system of step (1), continuing the reaction after the addition is completed, adding deionized water after the reaction is completed, and then adding an optional alkaline neutralizing agent to adjust the pH value of the system to neutral, thereby obtaining the aqueous polymer dispersant.

[0035] Preferably, the heating in step (1) is to 60-80°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, etc.

[0036] Preferably, the heating in step (1) is carried out under stirring conditions.

[0037] Preferably, the stirring speed is 280-320 r / min, for example, 280 r / min, 290 r / min, 300 r / min, 310 r / min, 320 r / min, etc.

[0038] Preferably, the heating in step (1) is carried out under an inert atmosphere.

[0039] Preferably, the inert atmosphere comprises nitrogen.

[0040] Preferably, the adding method in step (2) includes dropwise addition.

[0041] Preferably, the dropping time is 0.5 to 1.5 h, such as 0.5 h, 1 h, 1.5 h, etc.

[0042] Preferably, the continued reaction time is 1 to 3 hours, for example, 1 hour, 1.5 hours, 2 hours, 2.5 hours, 3 hours, etc.

[0043] Preferably, the amount of deionized water added in step (2) is such that the solid content of the system is 20% to 40%, for example, 20%, 22%, 24%, 26%, 28%, 30%, 32%, 34%, 36%, 38%, 40%, etc.

[0044] In actual operation, the present invention can adopt the following preparation method:

[0045] 1) According to the experimental plan, add all the base materials (polyoxyethylene ether monomers, additives) into a four-necked bottle; add the dropwise raw materials (monomers, chain transfer agents) into the corresponding conical flasks or beakers, seal them with rubber stoppers or sealing films, and insert silicone tubes;

[0046] 2) Turn on the water bath or oil bath, set the temperature (60-80°C) according to the experimental design, and turn on the cooling water;

[0047] 3) Turn on the mechanical stirrer, set the stirring speed to 280-320 rpm, and introduce N2;

[0048] 4) When the base material is completely dissolved and the temperature of the reaction material in the four-necked bottle reaches the set temperature, the initiator is added, the reaction starts, and the peristaltic pump parameters are set according to the experimental plan and turned on for dropwise addition;

[0049] 5) During the reaction, observe the changes in the temperature and viscosity of the material in the four-necked bottle and whether the droplet addition rate complies with the experimental plan;

[0050] 6) After the addition is completed, turn off the peristaltic pump;

[0051] 7) After reaching the set reaction time, add deionized water, and then add a measured amount of alkaline neutralizer to neutralize to neutrality;

[0052] 8) After the reaction is completed, turn off the water or oil bath to cool down, and keep the mechanical stirrer and cooling water on;

[0053] 9) After the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water, turn off the mechanical agitator, dismantle the reaction device, and transfer the material to the sample bottle.

[0054] It should be noted that the specific operation provided above is only an example, and the present invention is not limited to this specific operation.

[0055] The preparation method of the present invention is used to synthesize the aqueous polymer dispersant, which has the following advantages:

[0056] (1) No need to use solvents: The synthesis method of the present invention does not require the use of organic solvents, thus avoiding the problem of solvent removal caused by solution synthesis of traditional dispersants, thereby reducing both production costs and the risk of environmental pollution;

[0057] (2) Simplified synthesis process: The synthesis method of the present invention is simple and easy to implement, and does not require the use of special equipment, thereby reducing the difficulty and cost of production;

[0058] (3) Improving dispersant performance: The dispersant synthesized by the synthesis method of the present invention has a comb-like polymer structure. This structural feature makes it more effective in improving the stability of the coating and preventing the sedimentation and agglomeration of pigment particles, thereby improving the quality and performance of the coating;

[0059] (4) Environmentally friendly: The synthetic method of the present invention obtains an aqueous dispersant using water as a solvent, thereby avoiding the organic solvents used in traditional dispersants, thereby reducing the risk of environmental pollution and meeting current environmental protection requirements.

[0060] In the present invention, by adding additives, the mechanism of bulk polymerization process can be optimized:

[0061] ① When the added additives are in a finely dispersed state in the polymerization liquid, the polymerization heat can be quickly transferred to the additive droplets, thereby making the temperature of the polymerization liquid uniform, which is beneficial to improving product quality;

[0062] ② Part of the reactor is gas phase, and the evaporation of solvent and monomer to release polymerization heat is more efficient than the usual indirect heat exchange method;

[0063] ③ The additives dispersed in the polymer solution can reduce the apparent viscosity and reduce the stirring power consumption;

[0064] ④ Due to the presence of additives, the polymerization liquid is not easy to stick to the kettle.

[0065] In a third aspect, the present invention provides a use of the aqueous polymer dispersant as described in the first aspect in a coating.

[0066] The aqueous polymer dispersant provided by the present invention has good performance, can improve the stability of the coating, prevent the sedimentation and agglomeration of pigment particles, thereby improving the quality and performance of the coating, and can meet the current social demand for environmentally friendly, high-efficiency, and low-cost chemical products.

[0067] Compared with the prior art, the present invention has at least the following beneficial effects:

[0068] The aqueous polymer dispersant provided by the present invention does not contain organic solvents in its preparation raw materials, does not need to be subjected to solvent removal during the preparation process, is safe and environmentally friendly, and has a simple process; at the same time, by adopting macromolecular monomers (polyoxyethylene ether monomers) to provide side chains, introducing specific additives, and controlling their proportions, the problem of excessively high system viscosity occurring in bulk polymerization is solved; and by using the aqueous polymer dispersant in the preparation of coatings, the stability of the coatings can be improved, and the sedimentation and agglomeration of pigment particles can be prevented, thereby improving the quality and performance of the coatings. DETAILED DESCRIPTION

[0069] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0070] Unless otherwise specified, the experimental samples and reagents used in the following examples and comparative examples of the present invention are shown in Table 1 below.

[0071] Table 1

[0072] Serial number Sample / reagent name effect Specification Manufacturer 1 acrylic acid Anchoring Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 2 Fumaric Acid Anchoring Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 3 n-Butyl acrylate Hydrophobic Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 4 2-Ethylhexyl acrylate Hydrophobic Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 5 Styrene Hydrophobic Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 6 Octadecyl acrylate Hydrophobic Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 7 Isobornyl acrylate Hydrophobic Group 500mL / bottle Shanghai Aladdin Biochemical Technology Co., Ltd. 8 Ethyleneoxy Polyoxyethylene Ether 3000 Side chain group 1kg / bag Sailboat Petrochemical 9 Ethyleneoxypolyoxyethylene ether 600 Side chain groups 1kg / bag Sailboat Petrochemical 10 Azobisisobutyronitrile Initiator 500g / bottle Shanghai Titan Technology Co., Ltd. 11 3-Mercaptopropionic acid Chain transfer agent 500mL / bottle Shanghai Titan Technology Co., Ltd. 12 Dipropylene glycol butyl ether Additives 500mL / bottle Shanghai Titan Technology Co., Ltd. 13 Dipropylene glycol methyl ether Additives 500mL / bottle Shanghai Titan Technology Co., Ltd. 14 Ethylene glycol butyl ether Additives 500mL / bottle Shanghai Titan Technology Co., Ltd. 15 Xylene Solvents 500mL / bottle Shanghai Titan Technology Co., Ltd. 16 Isopropyl alcohol Solvents 500mL / bottle Shanghai Titan Technology Co., Ltd. 17 Sodium hydroxide Alkali 500mL / bottle Nanjing Chemical Reagent Co., Ltd.

[0073] The experimental instruments and equipment used in the present invention are shown in Table 2 below:

[0074] Table 2

[0075]

[0076]

[0077] Embodiment 1:

[0078] In this embodiment, an aqueous polymer dispersant is provided, and the preparation method comprises the following steps:

[0079] Take ethyleneoxy polyoxyethylene ether 3000 (165.0g, 0.055mol) and dipropylene glycol butyl ether (10.0g, 0.0526mol) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), pass nitrogen and heat to 70°C. Take acrylic acid (10.0g, 0.139mol), isooctyl acrylate (10.0g, 0.0543mol), and 3-mercaptopropionic acid (2.0g, 0.0188mol) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (0.5g, 0.003mol), turn on the peristaltic pump and set the drop time to 1h. After the drop addition is completed, continue the reaction for 2h. After the reaction is completed, add deionized water and adjust the solid content to 25%. Then add a measured amount of alkaline neutralizer (sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to neutrality. When the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water and mechanical stirrer, dismantle the reaction device, and transfer the material to the sample bottle.

[0080] Embodiment 2:

[0081] In this embodiment, an aqueous polymer dispersant is provided, and the preparation method comprises the following steps:

[0082] Take ethyleneoxy polyoxyethylene ether 3000 (60.0g, 0.02mol), ethyleneoxy polyoxyethylene ether 600 (5.0g, 0.0083mol) and dipropylene glycol butyl ether (20.0g, 0.105mol) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), introduce nitrogen and heat to 60°C. Separately take acrylic acid (14.0g, 0.194mol), isooctyl acrylate (12.0g, 0.0651mol), styrene (1.5g, 0.0144mol), 3-mercaptopropionic acid (2.0g, 0.0188mol) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 60°C, add azobisisobutyronitrile (0.4g, 0.0024mol), turn on the peristaltic pump and set the dropping time to 0.5h. After the dropwise addition is completed, continue the reaction for 1h. After the reaction is completed, add deionized water and adjust the solid content to 25%. Then add a measured amount of alkaline neutralizer (aqueous sodium hydroxide solution with a mass concentration of 25%) and neutralize to neutral. When the temperature of the material in the four-necked flask drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to the sample bottle.

[0083] Embodiment 3:

[0084] In this embodiment, an aqueous polymer dispersant is provided, and the preparation method comprises the following steps:

[0085] Take ethyleneoxy polyoxyethylene ether 3000 (115.0g, 0.0383mol), ethyleneoxy polyoxyethylene ether 600 (10.0g, 0.0167mol) and dipropylene glycol methyl ether (50.0g, 0.337mol) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), introduce nitrogen and heat to 80°C. Separately take acrylic acid (15.0g, 0.208mol), isobornyl acrylate (10.0g, 0.048mol), styrene (2.0g, 0.0192mol), fumaric acid (1.0g, 0.0086mol) and 3-mercaptopropionic acid (1.5g, 0.0141mol) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 80°C, add azobisisobutyronitrile (1.0g, 0.0061mol), turn on the peristaltic pump and set the dropping time to 1.5h. After the dropwise addition is completed, continue the reaction for 3h. After the reaction is completed, add deionized water and adjust the solid content to 25%. Then add a measured amount of alkaline neutralizer (aqueous sodium hydroxide solution with a mass concentration of 25%) and neutralize to neutral. When the temperature of the material in the four-necked flask drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to the sample bottle.

[0086] Embodiment 4:

[0087] In this embodiment, an aqueous polymer dispersant is provided, and the preparation method comprises the following steps:

[0088] Take ethyleneoxy polyoxyethylene ether 3000 (90.0g, 0.03mol), ethyleneoxy polyoxyethylene ether 600 (36.0g, 0.06mol) and ethylene glycol butyl ether (18.0g, 0.152mol) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), introduce nitrogen and heat to 70°C. Separately take acrylic acid (23.0g, 0.319mol), octadecyl acrylate (4.0g, 0.0123mol), styrene (2.0g, 0.0192mol) and 3-mercaptopropionic acid (1.5g, 0.0141mol) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (1.0g, 0.0061mol), turn on the peristaltic pump and set the dropping time to 1h. After the dropwise addition is completed, continue the reaction for 2h. After the reaction is completed, add deionized water and adjust the solid content to 25%. Then add a measured amount of alkaline neutralizer (aqueous sodium hydroxide solution with a mass concentration of 25%) and neutralize to neutral. When the temperature of the material in the four-necked flask drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to the sample bottle.

[0089] Comparative Example 1:

[0090] In this comparative example, a polymer dispersant is provided, and the preparation method comprises the following steps:

[0091] Take ethyleneoxy polyoxyethylene ether 3000 (100.61g, 0.0335mol), isooctyl acrylate (6.16g, 0.0335mol) and xylene (20.0g) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), pass nitrogen and heat to 70°C. Take acrylic acid (4.82g, 0.0669mol), isooctyl acrylate (6.16g, 0.0334mol), 3-mercaptopropionic acid (0.75g, 0.0071mol) and xylene (10.0g) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (2.25g, 0.0137mol), turn on the peristaltic pump and set the drop time to 1h. After the addition is complete, continue the reaction for 2 hours. Then remove the reaction solvent by rotary evaporator, add deionized water, and adjust the solid content to 25%. Finally, add a measured amount of alkaline neutralizer (a sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to a neutral reaction. When the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to a sample bottle.

[0092] Comparative Example 2:

[0093] In this comparative example, a polymer dispersant is provided, and the preparation method comprises the following steps:

[0094] Take ethyleneoxy polyoxyethylene ether 3000 (161.0g, 0.0537mol), isooctyl acrylate (2.45g, 0.0133mol) and xylene (32.7g) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), introduce nitrogen and heat to 70°C. Take acrylic acid (3.85g, 0.0534mol), isooctyl acrylate (2.45g, 0.0133mol), 3-mercaptopropionic acid (0.90g, 0.00848mol) and xylene (10g) in a 100mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (2.25g, 0.0137mol), turn on the peristaltic pump and set the drop time to 1h. After the addition is complete, continue the reaction for 2 hours. Then remove the reaction solvent by rotary evaporator, add deionized water, and adjust the solid content to 25%. Finally, add a measured amount of alkaline neutralizer (a sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to a neutral reaction. When the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to a sample bottle.

[0095] Comparative Example 3:

[0096] In this comparative example, a polymer dispersant is provided, and the preparation method comprises the following steps:

[0097] Take ethyleneoxy polyoxyethylene ether 3000 (30.25g, 0.01008mol), n-butyl acrylate (9.45g, 0.0734mol), acrylic acid (7.56g, 0.1049mol), 3-mercaptopropionic acid (2.0g, 0.0188mol) and isopropanol (116.04g) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), and introduce nitrogen. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (0.47g, 0.0029mol) and continue the reaction for 3h. Then remove the reaction solvent by a rotary evaporator, add deionized water, and adjust the solid content to 25%. Finally, add a measured amount of alkali neutralizer (sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to neutrality. When the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water and mechanical agitator, dismantle the reaction device, and transfer the material to the sample bottle.

[0098] Comparative Example 4:

[0099] In this comparative example, a polymer dispersant is provided, and the preparation method comprises the following steps:

[0100] Take acrylic acid (28.83g, 0.4mol), styrene (18.43g, 0.176mol), 3-mercaptopropionic acid (2.0g, 0.0188mol) and isopropanol (116.03g) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), and introduce nitrogen. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (0.47g, 0.0029mol) and continue the reaction for 3h. Then remove the reaction solvent by rotary evaporator, add deionized water, and adjust the solid content to 25%. Finally, add a measured amount of alkaline neutralizer (sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to neutrality. When the temperature of the material in the four-necked flask drops below 30°C, turn off the cooling water and mechanical stirrer, dismantle the reaction device, and transfer the material to the sample bottle.

[0101] Comparative Example 5:

[0102] In this comparative example, a polymer dispersant is provided, and the preparation method comprises the following steps:

[0103] Take ethyleneoxy polyoxyethylene ether 3000 (90.0g, 0.03mol) and styrene (1.56g, 0.015mol) in a 500mL four-necked flask, install a condenser and a thermometer, turn on the stirrer (300r / min), pass nitrogen and heat to 70°C. Take acrylic acid (9.37g, 0.13mol), styrene (1.56g, 0.015mol) and 3-mercaptopropionic acid (1.0g, 0.00942mol) in a 50mL conical flask, mix well, and connect a peristaltic pump. When the temperature of the reaction liquid in the four-necked flask reaches 70°C, add azobisisobutyronitrile (1.02g, 0.0062mol), turn on the peristaltic pump and set the drop time to 1h. After the drop addition is completed, continue the reaction for 2h. After the reaction is completed, add deionized water and adjust the solid content to 25%. Then add a measured amount of alkaline neutralizer (sodium hydroxide aqueous solution with a mass concentration of 25%) to neutralize to neutrality. When the temperature of the material in the four-necked bottle drops below 30°C, turn off the cooling water and mechanical stirrer, dismantle the reaction device, and transfer the material to the sample bottle.

[0104] The polymer dispersants provided in the examples and comparative examples were tested for performance, and the testing method was as follows:

[0105] 1. Determination of viscosity:

[0106] 1) Add 5.04 g of aqueous polymer dispersant to a stirring tank, add 108 g of water and stir at a low speed (stirring speed is 500 rpm) using a stirring abrasive dispersing multi-purpose machine;

[0107] 2) Slowly add 252g of titanium dioxide into the stirring tank at 500rpm. When the slurry becomes viscous and difficult to stir, increase the speed to 1000rpm and continue to add titanium dioxide, raising and lowering the stirring paddle from time to time to ensure uniform stirring;

[0108] 3) After all the titanium dioxide is added, stir at 1000 rpm for 5 minutes;

[0109] 4) When the slurry starts to flow, start testing its viscosity. When the slurry becomes more fluid, cover the mixing tank to prevent splashing. Use a viscosity tester to measure the viscosity. The initial parameters are: rotor: No. 64; speed: 60 rpm; time: 1 min.

[0110] 2. Determination of fineness

[0111] 1) Add 5.04g of water-based polymer dispersant to a dispersion tank, add 108g of water and stir at a low speed using a stirring sanding dispersing multi-purpose machine;

[0112] 2) Slowly add 252g of pigment (titanium dioxide) into the dispersant aqueous solution medium and stir at a speed of 500r / min for pre-wetting until there is no visible dry powder pigment in the container. Clean the pigment adhering to the container wall and the dispersion axis into the dispersion system and disperse for 5 minutes;

[0113] 3) Add zirconium beads, the amount of zirconium beads is 60% of the mass of the pigment water dispersion, sand grind at a speed of 3000r / min for 30min, and keep the temperature of the mixing system below 60°C during the dispersion process;

[0114] 4) According to GB / T 1724-79, the fineness of the pigment prepared above is measured.

[0115] The performance test results are shown in Table 3.

[0116] Table 3

[0117]

[0118]

[0119] It can be seen from Table 3 that, compared with the comparative example, when the aqueous polymer dispersant provided in the example of the present invention is used to disperse the pigment, the pigment has significantly lower viscosity (49.5-295 cp) and fineness (14-21 μm).

[0120] In summary, the synthesis method of the aqueous polymer dispersant provided by the present invention adopts a bulk polymerization system, does not introduce an organic solvent, does not require solvent removal, is safe and environmentally friendly, and has a simple process. At the same time, by using a macromolecular monomer to provide a side chain, introducing an auxiliary agent, and controlling its composition and proportion, the problem of excessively high system viscosity in bulk polymerization is solved.

[0121] The applicant declares that the present invention uses the above-mentioned embodiments to illustrate the aqueous polymer dispersant and its preparation method and application, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. An aqueous polymer dispersant, characterized in that The raw materials for preparing the aqueous polymer dispersant include the following components in parts by weight: The auxiliary agent includes any one of dipropylene glycol methyl ether, dipropylene glycol butyl ether, ethylene glycol butyl ether, diethylene glycol butyl ether, and dodecyl alcohol ester, or a combination of at least two of them.

2. The aqueous polymer dispersant according to claim 1, characterized in that The monomers include any one of acrylic acid, isooctyl acrylate, methacrylic acid, octadecyl acrylate, isobornyl acrylate, lauryl methacrylate, styrene, n-butyl acrylate, and fumaric acid, or a combination of at least two of them.

3. The aqueous polymer dispersant according to claim 1 or 2, characterized in that The polyoxyethylene ether monomers include ethyleneoxypolyoxyethylene ether; Preferably, the ethyleneoxy polyoxyethylene ether includes ethyleneoxy polyoxyethylene ether 3000 and / or ethyleneoxy polyoxyethylene ether 600.

4. The aqueous polymer dispersant according to any one of claims 1 to 3, characterized in that The initiator includes azobisisobutyronitrile; Preferably, the chain transfer agent comprises 3-mercaptopropionic acid.

5. The aqueous polymer dispersant according to any one of claims 1 to 4, characterized in that The raw materials for preparing the aqueous polymer dispersant also include an alkali neutralizer; Preferably, the alkaline neutralizing agent includes any one of ammonia water, sodium hydroxide solution, triethylamine, or a combination of at least two thereof; Preferably, the base neutralizer is used in an amount to adjust the pH value of the aqueous polymer dispersant to neutral.

6. The aqueous polymer dispersant according to any one of claims 1 to 5, characterized in that The solid content of the aqueous polymer dispersant is 20% to 40%.

7. A method for preparing an aqueous polymer dispersant as claimed in any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: (1) adding the formulated amount of polyoxyethylene ether monomer and auxiliary agent into a reactor, heating it, and then adding an initiator; (2) Mixing the monomer and the chain transfer agent, adding the obtained mixed solution to the system of step (1), continuing the reaction after the addition is completed, adding deionized water after the reaction is completed, and then adding an optional alkaline neutralizing agent to adjust the pH value of the system to neutral, thereby obtaining the aqueous polymer dispersant.

8. The preparation method according to claim 7, characterized in that: The heating in step (1) is to be raised to 60-80° C.; Preferably, the heating in step (1) is carried out under stirring; Preferably, the stirring speed is 280-320 r / min; Preferably, the heating in step (1) is carried out under an inert atmosphere; Preferably, the inert atmosphere comprises nitrogen.

9. The preparation method according to claim 7 or 8, characterized in that: The adding method in step (2) includes dropwise addition; Preferably, the dripping time is 0.5 to 1.5 hours; Preferably, the continued reaction time is 1 to 3 hours; Preferably, the amount of deionized water added in step (2) is such that the solid content of the system is 20% to 40%.

10. Use of the aqueous polymer dispersant according to any one of claims 1 to 6 in coatings.

Citation Information

Cited By

  • Ilmenite flotation dispersing agent, preparation method thereof and ilmenite flotation method

    CN120094748A