Mesoporous covalent organic framework material as well as preparation method and application thereof

Through the co-assembly of surfactants and covalent organic framework material precursors in the emulsion system, combined with pore reamers and catalysts, mesoporous covalent organic framework materials with adjustable pore size were prepared, and the micropores of covalent organic framework materials were solved. The problem of structural limitations performance has achieved the stability and wide application prospects of materials.

CN118930779APending Publication Date: 2024-11-12SHANGHAI UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310533453.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The microporous structure of existing covalent organic framework materials limits the accessibility of macromolecules, resulting in poor performance, and the steps to build multi-stage pore covalent organic framework materials through self-template and hard template strategies are cumbersome and pores are not connected. These problems have brought difficulties to the design and preparation of mesoporous covalent organic framework materials.

Method used

Co-assembly of surfactant and covalent organic skeleton material precursor in the emulsion system, the mesoporous covalent organic skeleton material is carried out by forming a two-phase interface and composite micelle, combining a pore reamer and a catalyst, and post-treatment is carried out to prepare mesoporous covalent organic skeleton material. , realize controllable adjustment of pore size, morphology and components.

Benefits of technology

The mesoporous covalent organic framework material with adjustable pore size was successfully prepared, which solved the problem of low mass transfer rate, and had stability and wide application prospects in the fields of catalysis, energy and biomedical.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930779A_ABST
    Figure CN118930779A_ABST
Patent Text Reader

Abstract

The invention relates to a mesoporous covalent organic framework material as well as a preparation method and application thereof, and the preparation method comprises the following steps: firstly, mixing a surfactant, a pore-enlarging agent and a solvent to form a two-phase interface and a compound micelle; adding a covalent organic framework material monomer, and forming a mesoporous covalent organic framework material precursor by utilizing self-assembly or interface assembly on an emulsion interface; and finally, adding the mesoporous covalent organic framework material precursor into a reaction solvent containing a catalyst, and carrying out post-treatment to obtain the mesoporous covalent organic framework material. Compared with the prior art, the preparation method is simple in process and good in repeatability, the prepared mesoporous covalent organic framework material has the advantages of being adjustable in size, controllable in morphology, good in stability and the like, mass transfer and load can be increased, the problems that currently synthesized small-hole and micropore covalent organic framework materials are low in mass transfer rate and the like are solved, and the application prospect is wide. Wide application prospects are realized in the fields of catalysis, energy sources, biomedicine and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of new materials and relates to a mesoporous covalent organic framework material and a preparation method and application thereof. Background Art

[0002] Covalent organic frameworks (COFs) are a class of organic porous crystalline nanomaterials mainly composed of light atoms such as C, H, N, B, and O, connected by covalent bonds. They have the characteristics of high crystallinity, large specific surface area, adjustable pore size, and functional modification. These properties give them unique properties, making them have good application prospects in applications such as catalysis, drug delivery, energy conversion, gas storage, and separation. However, the inherent micropores of most COFs hinder their mass transfer, limit the accessibility of macromolecules, and lead to poor performance. In order to cope with this limitation, it is meaningful and necessary to construct multi-level porous COFs.

[0003] The currently developed hierarchical pore covalent organic framework materials mainly include hollow covalent organic frameworks and macroporous covalent organic framework materials. They are mainly constructed by self-template and hard template strategies, with cumbersome steps and complex methods. At the same time, the obtained hierarchical pore covalent organic framework materials have problems such as unconnected pores and too thick pore walls. Ordered mesoporous structures have highly adjustable pore size and structure, which is expected to solve the above problems. In recent years, surfactant-based self-assembly strategies have been widely used in the synthesis of mesoporous metal oxides, mesoporous polymers and even mesoporous metal organic framework materials, and have achieved great success. However, the formation of covalent organic framework materials depends on the formation and correction of dynamic covalent bonds, which is different from the hydrolysis-crosslinking of metal oxides, the oligomerization-crosslinking of polymers, and the nucleation-growth formation process of metal organic framework materials. This makes its interaction with surfactants different, and it will greatly affect the self-assembly process of surfactants, which brings great difficulties to the design and preparation of mesoporous covalent organic framework materials. Therefore, developing a suitable strategy to prepare mesoporous covalent organic framework materials is a very valuable and challenging task. Summary of the invention

[0004] The purpose of the present invention is to provide a mesoporous covalent organic framework material and its preparation method and application. The present invention adopts an emulsion system to realize the preparation of mesoporous covalent organic framework material nanomaterials through the co-assembly of surfactants and covalent organic framework material precursors, and can realize controllable adjustment of pore size, morphology and components. The pore size of the obtained mesoporous covalent organic framework is 2 to 50 nm, the pore structure is spherical and branch-like, and the morphology is spherical and asymmetric bowl-shaped structure.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A method for preparing a mesoporous covalent organic framework material comprises the following steps:

[0007] S1: mixing surfactant, pore expander and solvent to form two-phase interface and composite micelles;

[0008] S2: adding covalent organic framework material monomers, and forming a mesoporous covalent organic framework material precursor by self-assembly or interface assembly at the emulsion interface;

[0009] S3: adding the mesoporous covalent organic framework material precursor into a reaction solvent containing a catalyst, and performing post-treatment to obtain the mesoporous covalent organic framework material.

[0010] Further, in step S1, the surfactant is a polyoxyethylene-b-polyoxypropylene-b-polyoxyethylene triblock copolymer Pluronic P123 (EO20PO70EO20), Pluronic F127 (EO106PO70EO106), Pluronic P103 (EO17PO56EO17), Pluronic P85 (EO26PO39EO26), Pluronic P65 (EO20PO30EO20), Pluronic L121 (EO5PO70EO5), Pluronic F88 (EO100PO39EO100), Pluronic F98 (EO123PO47EO123), Pluronic P105, Pluronic P84, Pluronic One or more combinations of F108 (EO132PO50EO132), PEO-b-PS or PEO-b-PMMA, the concentration of which in the mixture of surfactant, pore expander and solvent is 10 to 200 mg·mL -1 .

[0011] Furthermore, in step S1, the pore expanding agent is one or a combination of mesitylene, xylene, toluene, benzene, cyclohexane or n-hexane, and the amount used is 10% to 90% of the volume of the solvent.

[0012] Furthermore, in step S1, the solvent is one or a combination of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol or n-butanol;

[0013] When the solvent is a combination of multiple solvents and includes water, the volume ratio of water to other solvents is 1:100 to 100:1.

[0014] Further, in step S2, the covalent organic framework material monomer is one or more combinations of 1,3,5-benzenetricarboxaldehyde, 1,3,5-trialdehyde phloroglucinol, 2,5-dihydroxy-p-dibenzaldehyde, terephthalaldehyde, p-phenylenediamine, benzyl diamine, 2,5-diaminobenzenesulfonic acid, 2,3,5,6-tetrafluoro-1,4-phenylenediamine, 1,3,5-tris(4-aminophenyl)benzene or 2,4,6-tris(4-aminophenyl)-1,3,5-triazine;

[0015] The mass ratio of the covalent organic framework material monomer to the surfactant is 1:10 to 10:1.

[0016] Furthermore, in step S2, the self-assembly or interface assembly at the emulsion interface is: stirring at room temperature for 0.5 to 72 hours.

[0017] Further, in step S3, the reaction solvent is one or more combinations of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol, 1,3,5-trimethylbenzene, dichlorobenzene or n-butanol;

[0018] When the reaction solvents are a combination of two, the volume ratio of the two is 1:10-10:1.

[0019] Further, in step S3, the catalyst is one or more combinations of acetic acid, pyrrolidine, trifluoroacetic acid, p-toluenesulfonic acid or Sc(OTf)3;

[0020] The amount of the catalyst used is 1 to 20% of the volume of the reaction solvent;

[0021] The molar ratio of the catalyst to the covalent organic framework material monomer is 1-10000:1.

[0022] Further, in step S3, the post-treatment includes one of hydrothermal treatment, microwave hydrothermal treatment or supercritical CO2 treatment;

[0023] When hydrothermal treatment is used, the reaction temperature is 20 to 200°C and the reaction time is 1 to 72 hours;

[0024] When microwave hydrothermal treatment is adopted, the reaction temperature is 20-200°C, the reaction time is 1-72h, and the microwave power is 100-800W.

[0025] The invention discloses an application of a mesoporous covalent organic framework material, including applications in catalysis, energy or biomedicine.

[0026] Compared with the prior art, the present invention has the following characteristics:

[0027] 1) The present invention utilizes different solvents of the emulsion system to adjust the formation process of COF, promote the coordinated self-assembly of COF precursors and micelles, and obtain a mesoporous covalent organic framework material.

[0028] 2) The present invention utilizes an emulsion system to form a two-phase interface and micelles swollen by a pore-enlarging agent, which can adjust the mesopore diameter and mesopore structure, and the morphology of the mesoporous covalent organic framework material.

[0029] 3) The present invention utilizes a post-treatment method to improve the crystallinity of the mesoporous covalent organic framework material.

[0030] The preparation method of the present invention has simple process and good repeatability. The prepared mesoporous covalent organic framework material has the advantages of adjustable mesopore diameter (2-50nm), controllable pore structure (spherical and branched) and controllable morphology (spherical and asymmetric bowl-shaped structure), good stability, etc., which can increase mass transfer and load, solve the problem of low mass transfer rate of currently synthesized small pores and microporous covalent organic framework materials, and has broad application prospects in the fields of catalysis, energy, biomedicine, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is a scanning electron microscope image of the mesoporous covalent organic framework material prepared in Example 1;

[0032] Figure 2 This is a scanning electron microscope image of the asymmetric mesoporous covalent organic framework material prepared in Example 2;

[0033] Figure 3 This is a scanning electron microscope image of the branched mesoporous covalent organic framework material prepared in Example 3. DETAILED DESCRIPTION

[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] A mesoporous covalent organic framework material, including a spherical mesoporous covalent organic framework material and an asymmetric spherical covalent organic framework material, wherein the preparation method comprises the following steps:

[0036] S1: mixing surfactant, pore expander and solvent to form two-phase interface and composite micelles;

[0037] The surfactant is one or more combinations of Pluronic P123, P103, F108, F127, P105, P84, P85, L121, F98, PEO-b-PS or PEO-b-PMMA, and its concentration in the mixture of the surfactant, the pore expander and the solvent is 10 to 200 mg / mL;

[0038] The pore-enlarging agent is one or a combination of mesitylene, xylene, toluene, benzene, cyclohexane or n-hexane, and the amount used is 10%-90% of the volume of the solvent;

[0039] The solvent is one or more of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol or n-butanol; and when the solvent is a combination of multiple solvents and includes water, the ratio of the volume of water to the total volume of other solvents is 1:100 to 100:1;

[0040] S2: adding covalent organic framework material monomers, and forming a mesoporous covalent organic framework material precursor by self-assembly or interface assembly at the emulsion interface;

[0041] The monomer of the covalent organic framework material is one or more of 1,3,5-benzene trimeraldehyde, 1,3,5-trialdehyde phloroglucinol, 2,5-dihydroxy benzaldehyde, terephthalaldehyde, p-phenylenediamine, benzyl diamine, 2,5-diaminobenzenesulfonic acid, 2,3,5,6-tetrafluoro-1,4-phenylenediamine, 1,3,5-tris(4-aminophenyl)benzene or 2,4,6-tris(4-aminophenyl)-1,3,5-triazine, and the mass ratio of the monomer to the surfactant is 1:10 to 10:1;

[0042] The self-assembly or interfacial assembly at the interface of the emulsion is as follows: stirring at room temperature for 0.5 to 72 hours;

[0043] S3: adding a mesoporous covalent organic framework material precursor into a reaction solvent containing a catalyst, and performing post-treatment to obtain a mesoporous covalent organic framework material;

[0044] The reaction solvent is one or more of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol, 1,3,5-trimethylbenzene, dichlorobenzene or n-butanol; when the reaction solvent is a combination of two, the volume ratio of the two is 1:10-10:1;

[0045] The catalyst is one or more of acetic acid, pyrrolidine, trifluoroacetic acid, p-toluenesulfonic acid or Sc(OTf)3; the amount of the catalyst is 1-20% of the volume of the reaction solvent; the molar ratio of the catalyst to the covalent organic framework material monomer is 1-10000:1;

[0046] Post-treatment includes one of hydrothermal treatment, microwave hydrothermal treatment or supercritical CO2 treatment;

[0047] When hydrothermal treatment is used, the reaction temperature is 20 to 200°C and the reaction time is 1 to 72 hours;

[0048] When microwave hydrothermal treatment is adopted, the reaction temperature is 20-200°C, the reaction time is 1-72h, and the microwave power is 100-800W.

[0049] The invention discloses an application of a mesoporous covalent organic framework material, including applications in catalysis, energy or biomedicine.

[0050] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.

[0051] Embodiment 1:

[0052] Dissolve 1200mg F127 in 30mL dioxane, stir for 5min, add 30mL 1,3,5-trimethylbenzene and stir for 5min, then measure 30mL of deionized water and add it, stir for 5min. Then add 162mg 1,3,5-benzenetricarbaldehyde and 162mg p-phenylenediamine to the above solution, ultrasonicate at 200W for 5min, and stir at room temperature for 12h. Then centrifuge and wash repeatedly with ethanol and water for 6 times. Then add the precipitate after centrifugation to a mixed solution of 40mL 1,3,5-trimethylbenzene and 40mL dioxane, add 0.4mL 6M acetic acid to the above dispersion, and transfer it to a polytetrafluoroethylene liner, 120℃, and hydrothermal for three days. After taking it out, centrifuge and wash it repeatedly with ethanol and water for 6 times, and vacuum oven at 60℃ for 12h to obtain a spherical mesoporous covalent organic framework material ( Figure 1 ).

[0053] Embodiment 2:

[0054] Dissolve 1200mg F127 in 30mL dioxane, stir for 5min, add 40mL 1,3,5-trimethylbenzene and stir for 5min, then add 30mL deionized water and stir for 5min. Then add 162mg 1,3,5-benzenetricarbaldehyde and 162mg p-phenylenediamine to the above solution, ultrasonicate at 200W for 5min, and stir at room temperature for 12h. Then wash it by centrifugation repeatedly with ethanol and water for 6 times. Then add the precipitate after centrifugation to a mixed solution of 40mL 1,3,5-trimethylbenzene and 40mL dioxane, add 0.2mL trifluoroacetic acid to the above dispersion, transfer it to a polytetrafluoroethylene liner, and hydrothermal it at 120℃ and 400W microwave for 6h. After taking it out, wash it by centrifugation repeatedly with ethanol and water for 6 times, and vacuum oven at 60℃ for 12h to obtain an asymmetric mesoporous covalent organic framework material ( Figure 2 ).

[0055] Embodiment 3:

[0056] Dissolve 3000mg F127 in 30mL dioxane, stir for 5min, add 30mL 1,3,5-trimethylbenzene and stir for 5min, then measure 30mL of deionized water and add it, stir for 5min. Then add 162mg 1,3,5-benzenetricarbaldehyde and 162mg p-phenylenediamine to the above solution, ultrasonicate at 200W for 5min, and stir at room temperature for 12h. Then centrifuge and wash repeatedly with ethanol and water for 6 times. Then add the precipitate after centrifugation to 40mL 1,3,5-trimethylbenzene and 40mL dioxane mixed solution, add 0.4mL 6M acetic acid to the above dispersion, transfer to a polytetrafluoroethylene liner, and hydrothermal at 120℃ for three days. After taking out, centrifuge and wash repeatedly with ethanol and water for 6 times, and vacuum oven at 60℃ for 12h to obtain a dendritic mesoporous covalent organic framework material ( Figure 3 ).

[0057] Embodiment 4:

[0058] Dissolve 1200mg F127 in 30mL dioxane, stir for 5min, add 30mL 1,3,5-trimethylbenzene and stir for 5min, then add 30mL deionized water and stir for 5min. Then add 162mg 1,3,5-benzenetricarbaldehyde and 351mg 1,3,5-tri(4-aminophenyl)benzene to the above solution, ultrasonicate at 200W for 5min, and stir at room temperature for 12h. Then wash it by centrifugation repeatedly with ethanol and water for 6 times. Then add the precipitate after centrifugation to a mixed solution of 40mL dichlorobenzene and 40mL n-butanol, add 0.2mL pyrrolidine to the above dispersion, transfer it to a polytetrafluoroethylene liner, and hydrothermally heat it with microwaves at 120℃ and 400W for 6h. After taking it out, wash it by centrifugation repeatedly with ethanol and water for 6 times, and obtain a spherical mesoporous covalent organic framework material in a vacuum oven at 60℃ for 12h.

[0059] Embodiment 5:

[0060] Dissolve 1200mg F127 in 30mL dioxane, stir for 5min, add 30mL 1,3,5-trimethylbenzene and stir for 5min, then add 30mL deionized water and stir for 5min. Then add 351mg 1,3,5-tri(4-aminophenyl)benzene and 134mg terephthalaldehyde to the above solution, ultrasonicate at 200W for 5min, and stir at room temperature for 12h. Then wash it by centrifugation repeatedly with ethanol and water for 6 times. Then add the precipitate after centrifugation to a mixed solution of 40mL trimethylbenzene and 40mL dioxane, add 0.4mL 6M acetic acid to the above dispersion, and transfer it to a polytetrafluoroethylene liner, hydrothermal at 120℃ for three days. After taking it out, wash it by centrifugation repeatedly with ethanol and water for 6 times, and vacuum oven at 60℃ for 12h to obtain a spherical mesoporous covalent organic framework material.

[0061] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a mesoporous covalent organic framework material, characterized in that: The following steps are involved: S1: mixing surfactant, pore expander and solvent to form two-phase interface and composite micelles; S2: adding covalent organic framework material monomers, and forming a mesoporous covalent organic framework material precursor by self-assembly or interface assembly at the emulsion interface; S3: adding the mesoporous covalent organic framework material precursor into a reaction solvent containing a catalyst, and performing post-treatment to obtain the mesoporous covalent organic framework material.

2. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S1, the surfactant is one or more combinations of polyoxyethylene-b-polyoxypropylene-b-polyoxyethylene triblock copolymers Pluronic P123, Pluronic F127, Pluronic P103, Pluronic P85, Pluronic P65, Pluronic P105, Pluronic P84, Pluronic L121, Pluronic F88, Pluronic F98, Pluronic F108 PEO-b-PS or PEO-b-PMMA, and its concentration in the mixture of surfactant, pore expander and solvent is 10 to 200 mg·mL -1 .

3. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S1, the pore-enlarging agent is one or a combination of mesitylene, xylene, toluene, benzene, cyclohexane or n-hexane, and the amount used is 10% to 90% of the volume of the solvent.

4. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S1, the solvent is one or a combination of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol or n-butanol; When the solvent is a combination of multiple solvents and includes water, the volume ratio of water to other solvents is 1:100 to 100:

1.

5. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S2, the covalent organic framework material monomer is one or more combinations of 1,3,5-benzenetricarboxaldehyde, 1,3,5-trialdehyde phloroglucinol, 2,5-dihydroxy-p-dibenzaldehyde, terephthalaldehyde, p-phenylenediamine, benzyl diamine, 2,5-diaminobenzenesulfonic acid, 2,3,5,6-tetrafluoro-1,4-phenylenediamine, 1,3,5-tris(4-aminophenyl)benzene or 2,4,6-tris(4-aminophenyl)-1,3,5-triazine; The mass ratio of the covalent organic framework material monomer to the surfactant is 1:10 to 10:

1.

6. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S2, the self-assembly or interface assembly at the emulsion interface is: stirring at room temperature for 0.5 to 72 hours.

7. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S3, the reaction solvent is one or a combination of water, dioxane, acetonitrile, dimethyl sulfoxide, ethylene glycol, 1,3,5-trimethylbenzene, dichlorobenzene or n-butanol; When the reaction solvents are a combination of two, the volume ratio of the two is 1:10-10:

1.

8. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S3, the catalyst is one or more of acetic acid, pyrrolidine, trifluoroacetic acid, p-toluenesulfonic acid or Sc(OTf)3; The amount of the catalyst used is 1 to 20% of the volume of the reaction solvent; The molar ratio of the catalyst to the covalent organic framework material monomer is 1-10000:

1.

9. The method for preparing a mesoporous covalent organic framework material according to claim 1, characterized in that: In step S3, the post-treatment includes one of hydrothermal treatment, microwave hydrothermal treatment or supercritical CO2 treatment; When hydrothermal treatment is used, the reaction temperature is 20 to 200°C and the reaction time is 1 to 72 hours; When microwave hydrothermal treatment is adopted, the reaction temperature is 20-200°C, the reaction time is 1-72h, and the microwave power is 100-800W.

10. Use of a mesoporous covalent organic framework material prepared by the method according to any one of claims 1 to 9, characterized in that: These include applications in catalysis, energy or biomedicine.

Citation Information

Patent Citations

  • Large-aperture mesoporous nanoparticles and preparation method thereof

    CN102039132A

  • Method for preparing hierarchical porous UiO-66 material by using sodium dodecyl sulfonate as template

    CN110105581A

  • Preparation method and application of covalent organic framework material containing acylhydrazone bonds and disulfide bonds

    CN110183601A

  • COFs nanocrystal based on microemulsion template process, and preparation method and application thereof

    CN110437401A

  • Supported mesoporous MOF (at) COF composite porous particle as well as preparation method and application thereof

    CN115193405A