Prepreg resin paste and prepreg for preparing plate spring and preparation method of prepreg resin paste and prepreg
By strictly controlling the mixing ratio and preheating treatment of resin, curing agent and catalyst, the problem of insufficient fiber impregnation in the prepreg resin in the prior art is solved, and a prepreg with excellent dynamic mechanical properties is prepared, reducing pores defects improve mechanical properties.
Patent Information
- Application Number
- CN202310530182.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, when the prepreg is manufactured, the resin does not impregnate the fibers and the solvents are insufficiently removed, resulting in defects such as pores and significantly reduced dynamic mechanical properties.
By strictly controlling the mixing ratio of resin, curing agent and catalyst, preheating and mixing with reinforcing materials, a prepreg resin paste with excellent dynamic mechanical properties is prepared, including resin, curing agent and catalyst, with a resin content of 100 mass Fraction, the curing agent content is 10-25 mass fraction, the catalyst content is 2-8 mass fraction, the reinforcement material content is 60-70%, and the impregnation effect is ensured through preheating treatment and mixing accuracy control.
The good impregnation effect and excellent dynamic mechanical properties of the prepreg are achieved, reducing the pore defects of the product and improving the mechanical properties.
Smart Images

Figure CN118930815A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of composite materials, in particular to a prepreg resin paste and prepreg for preparing a leaf spring and a preparation method thereof. Background Art
[0002] Prepreg is a composite of resin matrix and reinforcement made by impregnating continuous fibers or fabrics with resin paste under strictly controlled conditions.
[0003] The method for manufacturing prepreg in the prior art generally adopts the powder prepreg method, which means that the resin powder is attached to the fiber, partially melted, and the resin is discontinuous, and the fiber is not fully impregnated with the resin. Other methods for manufacturing prepreg include solution impregnation, which means that the resin is dissolved in a solvent to make it a solution of a certain concentration, and then the fiber bundle or fabric passes through the resin matrix solution at a predetermined speed to make it impregnated with a certain amount of resin matrix, and then the solvent is removed by heating to finally form a prepreg.
[0004] The existing methods for manufacturing prepregs have a common defect, that is, the fibers are not fully impregnated with the obtained prepreg resin or the solvent in the prepreg is not fully removed. Most of the products made of such prepregs have defects such as pores, so their good dynamic mechanical properties are significantly reduced. Summary of the invention
[0005] The purpose of the embodiment of the present invention is to provide a prepreg with good impregnation effect and excellent dynamic mechanical properties to solve the problems in the prior art. The specific technical solution is as follows:
[0006] The embodiment of the present invention also provides a prepreg resin paste for preparing a leaf spring, the prepreg resin paste comprising: a resin, a curing agent and a catalyst;
[0007] The resin content is 100 mass fraction, the curing agent content is 10-25 mass fraction, and the catalyst content is 2-8 mass fraction.
[0008] Optionally, the resin is at least one of a polyphenol type glycidyl ether epoxy resin, a glycidyl ester epoxy resin and a glycidyl amine epoxy resin;
[0009] The curing agent is one of a polyamide curing agent, an aliphatic amine curing agent, an aromatic amine curing agent and a polyether amine curing agent;
[0010] The catalyst is one of ammonium persulfate, potassium persulfate, tetrabutylammonium bromide, triphenylphosphine, ethyltriphenylphosphine bromide and triethanolamine.
[0011] Optionally, the resin is specifically bisphenol A type solid epoxy resin; the curing agent is specifically polyamide curing agent; and the catalyst is specifically tetrabutylammonium bromide.
[0012] Optionally, the polyamide curing agent is prepared by condensation polymerization of dibasic fatty acid and polyamine.
[0013] The embodiment of the present invention also provides a prepreg for preparing a leaf spring, the prepreg comprising a prepreg resin paste and a reinforcing material;
[0014] The content of the prepreg resin paste is 30-40%, and the content of the reinforcing material is 60-70%; the prepreg resin paste is the prepreg resin paste described in the embodiment of the present invention.
[0015] Optionally, the reinforcing material is at least one of glass fiber, carbon fiber, and basalt fiber.
[0016] Optionally, the reinforcing material is specifically glass fiber.
[0017] The present invention also provides a method for preparing a prepreg, the method comprising:
[0018] The resin is subjected to a first preheating treatment to obtain a preheated resin;
[0019] The curing agent is subjected to a second preheating treatment to obtain a preheated curing agent;
[0020] The catalyst is subjected to a third preheating treatment to obtain a preheated catalyst;
[0021] Mechanically mixing the preheated resin, the preheated curing agent and the preheated catalyst to obtain a prepreg resin paste;
[0022] Mixing the prepreg resin paste and reinforcing material to obtain a prepreg;
[0023] Wherein, the first preheating treatment condition includes: temperature of 80-100°C, the second preheating treatment condition includes: 25-30°C, and the third preheating treatment condition includes: 25-30°C.
[0024] Optionally, the method further includes:
[0025] The prepreg is rolled up and cut to obtain a prepreg roll, and the prepreg roll is stored in an environment of 4-8°C.
[0026] In the embodiment of the present invention, a prepreg resin paste can be obtained by strictly controlling the accuracy of the mixing ratio of the resin, the curing agent and the catalyst, and then mixed with the reinforcing material and preheated to obtain a prepreg with good dynamic mechanical properties and high impregnation effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0028] Figure 1 A first schematic flow chart of a method for preparing a prepreg provided by an embodiment of the present invention;
[0029] Figure 2 A second schematic flow chart of a method for preparing a prepreg provided by an embodiment of the present invention;
[0030] Figure 3 A third schematic flow chart of a method for preparing a prepreg provided by an embodiment of the present invention;
[0031] Figure 4 A fourth flow chart of a method for preparing a prepreg provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0033] It should be noted that, in the absence of conflict, the features in the embodiments of the present invention may be combined with each other.
[0034] The embodiment of the present invention first provides a prepreg resin paste, wherein the prepreg resin paste comprises: a resin, a curing agent and a catalyst;
[0035] The resin content is 100 mass fraction, the curing agent content is 10-25 mass fraction, and the catalyst content is 2-8 mass fraction.
[0036] Specifically, the resin is at least one of polyphenol-type glycidyl ether epoxy resin, glycidyl ester epoxy resin and glycidyl amine epoxy resin; the curing agent is one of polyamide curing agent, aliphatic amine curing agent, aromatic amine curing agent and polyether amine curing agent; the catalyst is one of ammonium persulfate, potassium persulfate, tetrabutylammonium bromide, triphenylphosphine, ethyltriphenylphosphine bromide and triethanolamine.
[0037] More specifically, the resin is bisphenol A type solid epoxy resin; the curing agent is polyamide curing agent; and the catalyst is tetrabutylammonium bromide.
[0038] Wherein, the polyamide curing agent is prepared by polycondensation of dibasic fatty acid and polyamine.
[0039] The embodiment of the present invention further provides a prepreg for preparing a leaf spring, characterized in that the prepreg comprises a prepreg resin paste and a reinforcing material;
[0040] The content of the prepreg resin paste is 30-40%, and the content of the reinforcing material is 60-70%; the prepreg resin paste is the prepreg resin paste described in this embodiment.
[0041] Specifically, the reinforcing material is at least one of glass fiber, carbon fiber and basalt fiber.
[0042] More specifically, the reinforcing material is glass fiber.
[0043] Embodiment 1
[0044] The embodiment of the present invention further provides a method for preparing a prepreg. The following describes a method for preparing a prepreg provided by the embodiment of the present invention in conjunction with the accompanying drawings.
[0045] Embodiment 1
[0046] See also Figure 1 , Figure 1 The first process diagram of a method for preparing a prepreg provided by an embodiment of the present invention, wherein the prepreg comprises: a resin, a curing agent and a catalyst, such as Figure 1 As shown, the method comprises the following steps:
[0047] S110, performing a first preheating treatment on the resin to obtain a preheated resin;
[0048] Wherein, the first preheating treatment conditions include: the temperature is 80-100° C., and the resin content is 100 mass fraction.
[0049] Specifically, in practical applications, a preheating furnace can be used to perform a first preheating treatment on the resin. Before the first preheating treatment, the dirt on the resin barrel and its lid containing the resin can be cleaned first, and the resin barrel can be placed on the roller conveyor on the entrance side. The barrel lid is loosened, and the resin barrel automatically drives into the preheating furnace. The temperature of the preheating furnace is 80-100°C. After the first preheating treatment is completed, the resin barrel drives out of the preheating furnace to obtain preheated resin.
[0050] It can be understood that by performing the first preheating treatment on the resin, the mixing of the preheated resin can be better achieved and a predetermined prepreg result can be achieved subsequently.
[0051] S120, performing a second preheating treatment on the curing agent to obtain a preheated curing agent;
[0052] Wherein, the second preheating treatment conditions include: 25-30°C, and the curing agent content is 10-25 mass fraction.
[0053] Specifically, in practical applications, a preheating furnace can be used to perform a second preheating treatment on the curing agent. Before the second preheating treatment, the dirt on the curing agent container containing the curing agent can be cleaned first, and the curing agent container is placed on the roller conveyor on the entrance side. The cover of the curing agent container is loosened, and the curing agent container automatically enters the preheating furnace. The temperature of the preheating furnace is 25-30°C. After the second preheating treatment is completed, the curing agent container is driven out of the preheating furnace to obtain the preheated curing agent.
[0054] It can be understood that by performing a second preheating treatment on the curing agent, the mixing of the preheated curing agent can be better achieved and a predetermined pre-impregnation result can be achieved later.
[0055] S130, performing a third preheating treatment on the catalyst to obtain a preheated catalyst;
[0056] Wherein, the third preheating treatment conditions include: 25-30°C, and the catalyst content is 2-8 mass fractions.
[0057] Specifically, in practical applications, a preheating furnace can be used to perform a third preheating treatment on the catalyst. Before the third preheating treatment, the dirt on the catalyst container containing the catalyst can be cleaned first, and the catalyst container is placed on the roller conveyor on the inlet side. The catalyst container cover is loosened, and the catalyst container automatically drives into the preheating furnace. The temperature of the preheating furnace is 25-30°C. After the third preheating treatment is completed, the catalyst container drives out of the preheating furnace to obtain a preheated catalyst.
[0058] It can be understood that by performing the third preheating treatment on the catalyst, the mixing of the preheated catalyst can be better achieved and a predetermined pre-impregnation result can be achieved subsequently.
[0059] S140, adding the preheated curing agent to the preheated resin for mixing to obtain a mixture;
[0060] It should be noted that the preheated resin can be added into a designated mixer, and then the proportioned preheated curing agent is added into the preheated resin for mixing to obtain a mixture.
[0061] During the mixing process, the preheated resin and the preheated curing agent should be ensured to be fully mixed. Specifically, whether the mixing is uniform can be judged by observing the color of the inner wall and the bottom of the designated mixer. When the color of the inner wall and the bottom of the designated mixer is consistent with the color before adding the preheated resin and the preheated curing agent, that is, when the entire system after the preheated resin and the preheated curing agent are mixed is clear and transparent, it can be confirmed that the preheated resin and the preheated curing agent are fully mixed.
[0062] S150, adding the preheated catalyst into the mixture and mixing them to obtain a prepreg resin paste;
[0063] Specifically, after the preheating resin and the preheating curing agent are fully mixed, the preheating catalyst can be added to the mixed preheating resin and preheating curing agent to obtain the prepreg resin paste.
[0064] During the mixing process, the preheated resin, the preheated curing agent and the preheated catalyst should be ensured to be fully mixed. Specifically, whether the mixing is uniform can be judged by observing the color of the inner wall and the bottom of the mixer. When the color of the inner wall and the bottom of the mixer is consistent with the color before the preheated catalyst is added, that is, the entire system after the preheated resin, the preheated curing agent and the preheated catalyst are mixed is clear and transparent, it can be confirmed that the preheated resin, the preheated curing agent and the preheated catalyst are fully mixed.
[0065] S160, mixing the prepreg resin paste and the reinforcing material to obtain a prepreg;
[0066] In order to further improve the performance of the prepreg, in practical applications, the prepreg resin paste and reinforcing materials may be mixed to obtain the prepreg.
[0067] In practical applications, in order to obtain better dynamic mechanical properties of the prepared prepreg, the accuracy of the mixing ratio should be strictly controlled. It is understood that when the preheating resin, preheating curing agent and preheating catalyst are mixed, the maximum error allowed for the preheating resin is ±1% of the weight fraction, the maximum error allowed for the preheating curing agent is ±1% of the weight fraction, and the maximum error allowed for the preheating catalyst is ±0.5% of the weight fraction.
[0068] Specifically, the resin is bisphenol A type solid epoxy resin; the curing agent is polyamide curing agent; and the catalyst is tetrabutylammonium bromide.
[0069] In the embodiment of the present invention, by preheating the resin, curing agent and catalyst, and strictly controlling the accuracy of the mixing ratio of the preheated resin, preheated curing agent and preheated catalyst, a prepreg with good dynamic mechanical properties and high impregnation effect can be obtained.
[0070] Embodiment 2
[0071] See also Figure 2 , Figure 2 The second schematic diagram of the process for preparing a prepreg provided by an embodiment of the present invention, wherein the prepreg comprises: a resin, a curing agent and a catalyst, such as Figure 2 As shown, the method comprises the following steps:
[0072] S210, performing a first preheating treatment on the resin to obtain a preheated resin;
[0073] Wherein, the first preheating treatment conditions include: the temperature is 80-100° C., and the resin content is 100 mass fraction.
[0074] S220, performing a second preheating treatment on the curing agent to obtain a preheated curing agent;
[0075] Wherein, the second preheating treatment conditions include: 25-30°C, and the curing agent content is 10-25 mass fraction.
[0076] S230, performing a third preheating treatment on the catalyst to obtain a preheated catalyst;
[0077] Wherein, the third preheating treatment conditions include: 25-30°C, and the catalyst content is 2-8 mass fractions.
[0078] S240, confirming and recording the gel time of the preheated resin;
[0079] Specifically, in order to further improve the impregnation effect of the preheated resin, the gel time of the preheated resin may be confirmed and recorded.
[0080] The gel time of the preheated resin can be confirmed and recorded by taking a preset size of the preheated resin, placing it on a heating plate at a preset temperature, and continuously stirring it with a wooden stick until the preheated resin can be pulled into threads by the wooden stick. When the length of the thread formed by briefly pulling up the wooden stick reaches a preset length, the gel time of the preheated resin is confirmed and recorded.
[0081] More specifically, the preset size can be a circle with a diameter of 10 mm, the preset temperature is 130℃±2℃, and the preset length is at least 20 mm, that is, the preheated resin gel time is confirmed as: take a preheated resin sample with a diameter of 10 mm from the mixing head, place it on a heating plate at 130℃±2℃ and continue stirring with a wooden stick until the resin can be pulled into threads with a wooden stick, and when a thread of at least 20 mm long can be formed when the wooden stick is briefly pulled up, it is confirmed that the resin gel time has been reached.
[0082] Among them, the preheating resin gel time is 190-230s.
[0083] S250, adding the preheated curing agent to the preheated resin for mixing to obtain a mixture;
[0084] S260, adding the preheated catalyst into the mixture and mixing them to obtain a prepreg resin paste;
[0085] S270, mixing the prepreg resin paste and the reinforcing material to obtain a prepreg;
[0086] In the embodiment of the present invention, a prepreg having good dynamic mechanical properties and high impregnation effect is obtained by preheating the resin, curing agent and catalyst and strictly controlling the mixing ratio of the preheated resin, the preheated curing agent and the preheated catalyst. And by confirming the gel time of the preheated resin, the impregnation effect of the preheated resin is further improved.
[0087] Embodiment 3
[0088] See also Figure 3 , Figure 3 The third process diagram of a method for preparing a prepreg provided by an embodiment of the present invention, wherein the prepreg comprises: a resin, a curing agent and a catalyst, such as Figure 3 As shown, the method comprises the following steps:
[0089] S310, performing a first preheating treatment on the resin to obtain a preheated resin;
[0090] Wherein, the first preheating treatment conditions include: the temperature is 80-100° C., and the resin content is 100 mass fraction.
[0091] S320, performing a second preheating treatment on the curing agent to obtain a preheated curing agent;
[0092] Wherein, the second preheating treatment conditions include: 25-30°C, and the curing agent content is 10-25 mass fraction.
[0093] S330, performing a third preheating treatment on the catalyst to obtain a preheated catalyst;
[0094] Wherein, the third preheating treatment conditions include: 25-30°C, and the catalyst content is 2-8 mass fractions.
[0095] S340, confirming and recording the gel time of the preheated resin;
[0096] S350, adding the preheated curing agent to the preheated resin for mixing to obtain a mixture;
[0097] S360, adding the preheated catalyst into the mixture for mixing to obtain a prepreg resin paste;
[0098] S370, mixing the prepreg resin paste and the reinforcing material to obtain a prepreg;
[0099] S380, rolling up and cutting the prepreg to obtain a prepreg roll, and storing the prepreg roll in an environment of 4-8°C.
[0100] Specifically, in order to ensure that the mechanical properties of the prepreg are not weakened and to facilitate storage, the prepreg can be rolled and cut to obtain a prepreg roll, and the prepreg roll is stored in an environment of 4-8°C.
[0101] The storage period of the prepreg roll is greater than 12 hours and less than or equal to 21 days.
[0102] In practical applications, whether the prepared prepreg meets the requirements can be determined by determining the fiber content of the prepreg roll. Specifically, the prepreg roll can be cut into 0.5-meter strips, and the fiber content can be determined by performing a fiber content test on the 0.5-meter strips.
[0103] In the embodiment of the present invention, by preheating the resin, curing agent and catalyst, and strictly controlling the accuracy of the mixing ratio of the preheated resin, the preheated curing agent and the preheated catalyst, a prepreg with good dynamic mechanical properties and high impregnation effect is obtained. And by confirming the gel time of the preheated resin, the impregnation effect of the preheated resin is further improved. By winding and cutting the prepreg and controlling the storage environment, it is ensured that the mechanical properties of the prepreg are not weakened.
[0104] Embodiment 4
[0105] See also Figure 4 , Figure 4 A fourth flow diagram of a method for preparing a prepreg provided by an embodiment of the present invention, wherein the prepreg comprises: a resin, a curing agent and a catalyst, such as Figure 4 As shown, the method comprises the following steps:
[0106] S410, performing a first preheating treatment on the resin to obtain a preheated resin;
[0107] Wherein, the first preheating treatment conditions include: the temperature is 80-100° C., and the resin content is 100 mass fraction.
[0108] S420, performing a second preheating treatment on the curing agent to obtain a preheated curing agent;
[0109] Wherein, the second preheating treatment conditions include: 25-30°C, and the curing agent content is 10-25 mass fraction.
[0110] S430, performing a third preheating treatment on the catalyst to obtain a preheated catalyst;
[0111] Wherein, the third preheating treatment conditions include: 25-30°C, and the catalyst content is 2-8 mass fractions.
[0112] S440, confirming and recording the gel time of the preheated resin;
[0113] S450, adding the preheated curing agent to the preheated resin for mixing to obtain a mixture;
[0114] S460, adding the preheated catalyst into the mixture and mixing them to obtain a prepreg resin paste;
[0115] S470, mixing the prepreg resin paste and the reinforcing material to obtain a prepreg;
[0116] S480, rolling up and cutting the prepreg to obtain a prepreg roll, and storing the prepreg roll in an environment of 4-8° C.;
[0117] S490: affixing a label to the prepreg roll.
[0118] In order to facilitate the identification and control of the prepreg rolls, a label may be affixed to the prepreg rolls, wherein the label may include at least one of: roll number, production length, production date, storage temperature, storage period, and production personnel.
[0119] In the embodiment of the present invention, by preheating the resin, curing agent and catalyst, and strictly controlling the accuracy of the mixing ratio of the preheated resin, the preheated curing agent and the preheated catalyst, a prepreg with good dynamic mechanical properties and high impregnation effect is obtained. And by confirming the gel time of the preheated resin, the impregnation effect of the preheated resin is further improved. By winding and cutting the prepreg and controlling the storage environment, it is ensured that the mechanical properties of the prepreg are not weakened. By affixing a label on the prepared prepreg roll, it is convenient to identify and control the prepreg.
[0120] Embodiment 5
[0121] An embodiment of the present invention provides a prepreg obtained by the prepreg preparation method provided by this embodiment.
[0122] Specifically, 100 mass fractions of resin, 15 mass fractions of curing agent, and 5 mass fractions of catalyst are taken.
[0123] First, 100 mass fractions of resin are subjected to a first preheating treatment at a temperature of 90° C. in a designated container to obtain a preheated resin; then, 15 mass fractions of a curing agent are subjected to a second preheating treatment at a temperature of 28° C. in a designated container to obtain a preheated curing agent; then, 5 mass fractions of a catalyst are subjected to a third preheating treatment at a temperature of 28° C. in a designated container to obtain a preheated catalyst; the obtained preheated curing agent is added to the obtained preheated resin for mixing to obtain a mixture, and after sufficient mixing, the obtained preheated catalyst is added to the obtained mixture for mixing to obtain a prepreg resin paste.
[0124] The obtained prepreg resin paste and reinforcing material are mixed to obtain a prepreg, wherein the content of the prepreg resin paste is 35%, and the reinforcing material is specifically glass fiber, and the content of the glass fiber is 65%.
[0125] Embodiment 6
[0126] An embodiment of the present invention further provides a composite leaf spring, which is obtained by compression molding a prepreg, wherein the prepreg used is a prepreg prepared by any method provided in the embodiments of the present invention.
[0127] In practical applications, the mold temperature of the composite leaf spring can be 120°C. The prepreg prepared by any of the methods provided in this embodiment is placed in a mold, pressed, heated and cured, and taken out after cooling to obtain a composite leaf spring product. Specifically, the prepreg can be cured in an environment of 120°C-140°C for 30-60 minutes before demolding, so that the degree of curing reaches 95-97%, so as to obtain ideal dynamic performance and mechanical properties.
[0128] Specifically, in practical applications, a release agent can be used for demolding. The release agent is a liquid external release agent that does not contain silicon-based substances. It is suitable for mass production of composite materials for automobiles and can achieve rapid demolding. It can be used at the beginning of production or when re-production after cleaning the mold, which is very helpful in improving the demolding performance of the product. It can be used on a smooth mold surface. Especially when other types of release agents have been used, the mold surface should be thoroughly cleaned before use. It can also be diluted with deionized water before use.
[0129] The composite leaf spring provided in the embodiment of the present invention has good dynamic mechanical properties, a tensile strength of up to 1200 MPa, a bending modulus and a tensile modulus of up to 40-50 Gpa, high toughness, and is not prone to breakage during the experiment.
[0130] Each embodiment in this specification is described in a related manner, and the same or similar parts between the embodiments can be referenced to each other, and each embodiment focuses on the differences from other embodiments.
[0131] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the existence of other identical elements in the process, method, article or device including the elements.
[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the protection scope of the present invention. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention are included in the protection scope of the present invention.
Claims
1. A prepreg resin paste for leaf spring preparation, characterized in that: The prepreg resin paste comprises: resin, curing agent and catalyst; The resin content is 100 mass fraction, the curing agent content is 10-25 mass fraction, and the catalyst content is 2-8 mass fraction.
2. The prepreg resin paste according to claim 1, characterized in that The resin is at least one of a polyphenol type glycidyl ether epoxy resin, a glycidyl ester epoxy resin and a glycidyl amine epoxy resin; The curing agent is at least one of a polyamide curing agent, an aliphatic amine curing agent, an aromatic amine curing agent and a polyether amine curing agent; The catalyst is at least one of ammonium persulfate, potassium persulfate, tetrabutylammonium bromide, triphenylphosphine, ethyltriphenylphosphine bromide and triethanolamine.
3. The prepreg resin paste according to claim 2, characterized in that The resin is specifically bisphenol A type solid epoxy resin; the curing agent is specifically polyamide curing agent; and the catalyst is specifically tetrabutylammonium bromide.
4. The prepreg resin paste according to claim 3, characterized in that The polyamide curing agent is prepared by polycondensation of dibasic fatty acid and polyamine.
5. A prepreg for preparing a leaf spring, characterized in that: The prepreg comprises a prepreg resin paste and a reinforcing material; The content of the prepreg resin paste is 30-40%, and the content of the reinforcing material is 60-70%; the prepreg resin paste is the prepreg resin paste described in any one of claims 1-4.
6. The prepreg according to claim 5, characterized in that The reinforcing material is at least one of glass fiber, carbon fiber and basalt fiber.
7. The prepreg according to claim 6, characterized in that The reinforcing material is specifically glass fiber.
8. A method for preparing a prepreg, characterized in that: The method comprises: The resin is subjected to a first preheating treatment to obtain a preheated resin; The curing agent is subjected to a second preheating treatment to obtain a preheated curing agent; The catalyst is subjected to a third preheating treatment to obtain a preheated catalyst; adding the preheated curing agent into the preheated resin and mixing them to obtain a mixture; adding the preheated catalyst into the mixture and mixing them to obtain a prepreg resin paste; Mixing the prepreg resin paste and reinforcing material to obtain a prepreg; Wherein, the first preheating treatment condition includes: temperature of 80-100°C, the second preheating treatment condition includes: 25-30°C, and the third preheating treatment condition includes: 25-30°C.
9. The method according to claim 8, characterized in that The method further comprises: The prepreg is rolled up and cut to obtain a prepreg roll, and the prepreg roll is stored in an environment of 4-8°C.