Weather-resistant amorphous copolyester material and preparation method thereof

Through the combination of a supported catalyst and an amidine-based ultraviolet absorber, the crystallinity and dielectric loss of the copolyester material are reduced, the problems of insufficient weather resistance and thermal stability of the material in the prior art are solved, and high transparency and Electromagnetic compatibility, suitable for high-performance polyester applications.

CN118930824APending Publication Date: 2024-11-12HENAN YUANHONG POLYMER NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411235446.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing non-crystalline copolyester materials have limitations in weather resistance, thermal stability and mechanical properties, and are prone to degradation under ultraviolet irradiation and extreme temperature conditions, affecting their application under a wider range of environmental conditions.

Method used

The supported catalyst is used to form antimony-germanium nanoparticles through catalytic reaction of ionic liquid, combining amidine-based ultraviolet absorbers and alicyclic diols to reduce the crystallinity and dielectric loss of the material, and improve the disorderly arrangement of the polyester chains and UV resistance.

Benefits of technology

It realizes high transparency and electromagnetic compatibility of weather-resistant non-crystalline copolyester materials, and is suitable for polyester heat shrink films and high transparent sheets, improving the market value and performance stability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027606240000041
    Figure BDA0005027606240000041
  • Figure BDA0005027606240000042
    Figure BDA0005027606240000042
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer materials, and provides a weather-resistant amorphous copolyester material and a preparation method thereof. The flame-retardant polyester resin is prepared from the following raw materials: 30 to 80 parts of terephthalic acid, 20 to 30 parts of ethylene glycol, 5 to 10 parts of neopentyl glycol, 10 to 20 parts of alicyclic dihydric alcohol, 0.05 to 0.25 part of a supported catalyst, 0.01 to 0.2 part of a stabilizer, 2 to 5 parts of an amidine ultraviolet light absorber and 0.5 to 1 part of an antioxidant. The copolyester material disclosed by the invention belongs to amorphous polyester, can be applied to the fields of polyester heat shrinkage films and high-transparency plates and sheets, and has better market value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials, and in particular relates to a weather-resistant non-crystalline copolyester material and a preparation method thereof. Background Art

[0002] With the rapid development of modern industry, non-crystalline copolyester materials have been widely used in plastic products, packaging materials, textile fibers and other fields due to their light weight, durability and excellent processing performance. However, existing materials have certain limitations in weather resistance, thermal stability and mechanical properties, which restricts their application in a wider range of environmental conditions. In the field of plastic products, weather resistance is a key indicator to measure the service life of materials. Traditional non-crystalline copolyester materials are easily degraded under ultraviolet radiation and extreme temperature conditions, resulting in performance degradation.

[0003] Chinese patent CN 117510810 A discloses a PBAT-ETL copolyester material with high elongation at break and its preparation method. The copolyester material is prepared from the following raw materials: adipic acid, 1,4-butanediol, terephthalic acid, erythritol, and tetrabutyl titanate; adipic acid, 1,4-butanediol, terephthalic acid, and erythritol are blended according to the ratio without adding a catalyst, and successively undergo two-step esterification and polycondensation to obtain the PBAT-ETL copolyester material; the synthesis method provided by the present invention improves the elongation at break and has biodegradability. However, the use of 1,4-butanediol may have the risk of crystallization, which affects the processing and transparency of the copolyester material and has limited application areas.

[0004] Therefore, there is an urgent need to develop a weather-resistant non-crystalline copolyester material that has good weather resistance and is not easy to crystallize. Summary of the invention

[0005] In view of the existing technical problems, the purpose of the present invention is to provide a weather-resistant non-crystalline copolyester material and a preparation method thereof. The copolyester material of the present invention belongs to non-crystalline polyester, can be applied to the fields of polyester heat shrinkable film and high-transparency sheet material, and has good market value.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] On the one hand, the present invention provides a weather-resistant non-crystalline copolyester material, which comprises the following raw materials, by weight: 30-80 parts of terephthalic acid, 20-30 parts of ethylene glycol, 5-10 parts of neopentyl glycol, 10-20 parts of alicyclic diols, 0.05-0.25 parts of supported catalysts, 0.01-0.2 parts of stabilizers, 2-5 parts of amidine ultraviolet absorbers, and 0.5-1 parts of antioxidants.

[0008] The reaction mechanism of the present invention is as follows:

[0009] 1. The catalyst of the present invention is a supported catalyst. By introducing the ionic liquid 1-aminoethyl-3-methylimidazolium tetrafluoroborate, the epoxy group on the graphene oxide and the amino group on the ionic liquid undergo a nucleophilic ring-opening reaction under the catalytic action of potassium hydroxide, and the positively charged imidazole ring in the ionic liquid is grafted onto the graphene oxide. On the one hand, the stacking and overlapping of the graphene oxide are effectively prevented, and the specific surface area of ​​the graphene oxide is increased; on the other hand, when ethylene glycol antimony and tetrabutoxygermanium are added, the electrostatic force between the anions and cations can make the ethylene glycol antimony and tetrabutoxygermanium uniformly dispersed on the graphene oxide; at the same time, the applicant unexpectedly found that the metal compound will spontaneously undergo a redox reaction under ultrasound, thereby generating antimony-germanium nanoparticles deposited on the graphene oxide, which may be due to the redox potential difference between ethylene glycol antimony, tetrabutoxygermanium and graphene oxide.

[0010] Furthermore, in the present invention, by adding a reducing agent, graphene oxide will be subjected to the interaction of hydrogen bonds and π-π bonds between sheets under hydrothermal reduction conditions, thereby forming a final stable supported catalyst with good catalytic activity, which can promote the disordered arrangement of polyester chains, thereby reducing crystallinity.

[0011] 2. Ultraviolet absorbers are polymer weathering additives. Currently, there are mainly benzotriazole ultraviolet absorbers, benzophenone ultraviolet absorbers, and triazine ultraviolet absorbers. The three have their own unique absorption spectra and application performance, and play an important role in different fields. Both benzotriazole ultraviolet absorbers and triazine ultraviolet absorbers may cause color changes in certain polyester materials, affecting the transparency and color of the materials; benzophenone ultraviolet absorbers can effectively absorb UV light, but their mobility in polyester materials may cause uneven protective layers, reducing their long-term protective effects. Compared with the above-mentioned ultraviolet absorbers, formamidine ultraviolet absorbers play a role in polyester materials that cannot be replaced by other ultraviolet absorbers.

[0012] As nucleophiles, carboxamidine derivatives attack the chloromethyl group of 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene. The presence of fluorine atoms may increase the electropositivity of the chloromethyl group, making it more susceptible to nucleophilic attack and more prone to nucleophilic substitution reactions, forming a conjugated structure with ultraviolet absorption ability. Secondly, the synthesized amidine ultraviolet absorber has a symmetrical structure, which can provide a better conjugation effect and improve the polymer's ability to absorb ultraviolet light and thermal stability. In addition, due to the high electronegativity of fluorine atoms, fluorine-containing polymers can enhance the polymer's anti-ultraviolet performance. The introduction of fluorine atoms may change the transition mode of electrons in the polymer, thereby affecting its absorption of ultraviolet rays.

[0013] 3. The present invention adds alicyclic diols, whose cyclic structures can introduce more symmetry into the polymer chains, thereby helping to reduce the regular arrangement of the polymer chains and reduce the crystallinity of the materials, so that the materials can adapt to different industrial applications. In addition, when alicyclic diols are introduced into copolyesters, they will replace part of the terephthalic acid units, thereby reducing the number of ester groups, thereby reducing the polarizability of the polymer chains, reducing the dielectric loss of the materials in the AC electric field, and further improving the insulation properties and electromagnetic compatibility of products such as transparent sheet materials.

[0014] In some embodiments, the method for preparing the supported catalyst comprises the following steps:

[0015] S1. Graphene oxide is dispersed in deionized water, 1-aminoethyl-3-methylimidazolium tetrafluoroborate is added, the mixture is poured into a reaction kettle, potassium hydroxide is added, and ultrasonic treatment is performed for 30-45 minutes to obtain a mixture containing an ionic liquid;

[0016] S2. The mixture containing the ionic liquid obtained in step S1, antimony glycol and tetrabutoxygermanium were added to the reactor, ultrasonically treated for 30-45 min, and stirred for 12-16 h to obtain a mixed solution;

[0017] S3. Add a reducing agent to the mixed solution obtained in step S2, stir for 20-30 minutes, dry at 80-90° C. for 5-6 hours, cool to room temperature, wash, and obtain a supported catalyst.

[0018] In some embodiments, the mass ratio of graphene oxide to 1-aminoethyl-3-methylimidazolium tetrafluoroborate in step S1 is (0.5-0.8):1.

[0019] In some embodiments, the mass ratio of the reducing agent in step S3 to the graphene oxide in step S1 is (2.5-3):1.

[0020] Preferably, the mass ratio of antimony glycolate to germanium tetrabutoxide in step S2 is (2.6-3.2):1.

[0021] In some embodiments, the method for preparing the amidine ultraviolet absorber comprises the following steps:

[0022] Add N,N'-bis(4-ethoxycarbonylphenyl)formamidine and a composite organic solvent into a reaction kettle, stir to dissolve, add potassium carbonate under an inert gas protection atmosphere, heat to 60-80°C, keep warm for 0.5-1.5h, add 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene, heat to 90-120°C, keep warm for 2-5h, cool, rotary evaporate, and recrystallize to obtain a novel amidine ultraviolet absorber.

[0023] In some embodiments, the composite organic solvent is N,N-dimethylformamide and acetonitrile, and the volume ratio of the two is 1:(1.5-3).

[0024] In some embodiments, the molar ratio of N,N'-bis(4-ethoxycarbonylphenyl)formamidine to 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene is (2-2.5):1; wherein the structural formula of N,N'-bis(4-ethoxycarbonylphenyl)formamidine is as follows:

[0025]

[0026] Specifically, the amidine-based novel ultraviolet absorber has the following structural formula:

[0027]

[0028] In some embodiments, the antioxidant is any one or more of hindered phenols, hindered amines and phosphites.

[0029] In some embodiments, the alicyclic diol is any one or more of 1,4-cyclohexanedimethanol, tricyclodecane dimethanol and bicyclo[2.2.1]heptane-2,2-dimethanol.

[0030] Preferably, the alicyclic diol is 1,4-cyclohexanedimethanol.

[0031] Another aspect of the present invention provides a method for preparing a weather-resistant non-crystalline copolyester material, comprising the following steps:

[0032] 1. Put terephthalic acid, ethylene glycol, neopentyl glycol, alicyclic diol and supported catalyst into a beating kettle for mixing and beating to prepare slurry, and beat for 30-45 minutes, and then put it into an esterification reaction kettle 1 for esterification at normal pressure, and control the temperature in the kettle at 230-280° C. to obtain esterification liquid 1;

[0033] 2. Inert gas is introduced into the esterification reaction kettle 1, and the esterification liquid material 1 of step 1 is pressed into the esterification reaction kettle 2. The amidine ultraviolet absorber and antioxidant are mixed together with the stabilizer and put into the kettle and stirred for 10-20 minutes. The temperature in the kettle is controlled at 220-260° C. to obtain the esterification liquid material 2;

[0034] 3. The esterified liquid material 2 of step 2 is introduced into an inert gas and pressed into a polycondensation reaction kettle. When heated to 260-280°C, the pressure is pumped down to less than 1KPa by stirring. The temperature is controlled at 280-295°C. The reaction is carried out for 1-2h. The vacuum jet pump is turned on. The pressure in the kettle reaches 50-80Pa. The reaction time is 3.5-5h. The material is discharged, pelletized and dried to obtain a copolyester material.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] 1. The copolyester material of the present invention is a non-crystalline polyester, which can be applied to the fields of polyester heat shrinkable films and highly transparent sheet materials, and has good market value.

[0037] 2. The catalyst of the present invention is a supported catalyst. The ionic liquid 1-aminoethyl-3-methylimidazolium tetrafluoroborate effectively prevents the stacking and overlapping of graphene oxide, increases the specific surface area of ​​graphene oxide and has good stability. There may be a redox potential difference between ethylene glycol antimony, tetrabutoxygermanium and graphene oxide, which converts them into nanoparticles. At the same time, the addition of a reducing agent further improves the thermal stability of the supported catalyst, has good catalytic activity, promotes the disordered arrangement of polyester chains, and thus reduces crystallinity.

[0038] 3. The amidine ultraviolet absorber of the present invention forms a conjugated structure with ultraviolet absorption ability, and its symmetrical structure can provide a better conjugation effect, thereby improving the ultraviolet absorption ability and thermal stability of the polymer.

[0039] 4. The addition of alicyclic diols in the present invention reduces the crystallinity and dielectric loss of the material, making the material adaptable to different industrial applications. DETAILED DESCRIPTION

[0040] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0041] According to the ratios of the raw materials and the preparation methods specified in the following examples and comparative examples, various copolyester materials were prepared.

[0042] The raw materials used in the examples and comparative examples are not specifically mentioned and can be purchased from the market.

[0043] Preparation Example 1

[0044] The preparation method of supported catalyst A comprises the following steps:

[0045] S1. 200 mg of graphene oxide was dispersed in 100 ml of deionized water, 130 mg of 1-aminoethyl-3-methylimidazolium tetrafluoroborate was added, the mixture was poured into a reaction vessel, 254 g of potassium hydroxide was added, and the mixture was ultrasonically treated for 40 min to obtain a mixture containing an ionic liquid;

[0046] S2. 560 mg of the ionic liquid-containing mixture obtained in step S1, 10.5 mg of ethylene glycol antimony and 3.5 mg of tetrabutoxygermanium were added to the reactor, ultrasonically treated for 40 min, and stirred for 16 h to obtain a mixed solution;

[0047] S3. Add 0.56 g of hydroxylamine hydrochloride to the mixed solution obtained in step S2, stir for 30 min, dry at 80° C. for 6 h, cool to room temperature, and wash with ethanol and deionized water three times each to obtain supported catalyst A.

[0048] Preparation Example 2

[0049] The preparation method of supported catalyst B is the same as that of Preparation Example 1, except that the added amount of 1-aminoethyl-3-methylimidazolium tetrafluoroborate is 80 mg.

[0050] Preparation Example 3

[0051] The preparation method of supported catalyst C is the same as that of Preparation Example 1, except that the amount of hydroxylamine hydrochloride added is 0.4 g.

[0052] Preparation Example 4

[0053] The preparation method of amidine ultraviolet absorber A comprises the following steps:

[0054] 10 mmol of N,N'-bis(4-ethoxycarbonylphenyl)formamidine, 40 ml of N,N-dimethylformamide and 80 ml of acetonitrile were added into a reaction kettle and stirred for 1 hour to dissolve. Under a nitrogen atmosphere, 12 mmol of potassium carbonate was added, the temperature was raised to 70°C and kept warm for 1 hour, 4.5 mmol of 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene was added, the temperature was raised to 100°C, the temperature was kept warm for 4 hours, the mixture was cooled to 30°C, rotary evaporated and recrystallized with ethanol to obtain a novel amidine ultraviolet absorber A.

[0055] Preparation Example 5

[0056] The preparation method of amidine ultraviolet absorber B is the same as that of Preparation Example 4, except that 120 ml of N,N-dimethylformamide is added instead of 40 ml of N,N-dimethylformamide and 80 ml of acetonitrile.

[0057] Preparation Example 6

[0058] The preparation method of amidine ultraviolet absorber C is the same as that of Preparation Example 4, except that 6.75 mmol of N,N'-bis(4-ethoxycarbonylphenyl)formamidine is added.

[0059] Example 1

[0060] A weather-resistant non-crystalline copolyester material comprises the following raw materials, measured by weight: 55 parts of terephthalic acid, 25 parts of ethylene glycol, 7.5 parts of neopentyl glycol, 15 parts of 1,4-cyclohexanedimethanol, 0.15 parts of supported catalyst A, 0.1 parts of trimethyl phosphate, 3.5 parts of amidine ultraviolet absorber A, and 0.75 parts of antioxidant 1010.

[0061] The preparation method of the copolyester material of this embodiment comprises the following steps:

[0062] 1. Put terephthalic acid, ethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol and supported catalyst A into a beating kettle for mixing and beating to prepare slurry, and beat for 38 minutes. Then, send them into esterification reaction kettle 1 through a screw slurry delivery pump for normal pressure esterification. The temperature in the kettle is controlled at 255° C. to obtain esterification liquid 1;

[0063] 2. Nitrogen is introduced into the esterification reaction kettle 1, and the esterification liquid material 1 of step 1 is pressed into the esterification reaction kettle 2. The amidine ultraviolet absorber A and the antioxidant 1010 are mixed and put into the kettle together with trimethyl phosphate and stirred for 15 minutes. The temperature in the kettle is controlled at 240° C. to obtain the esterification liquid material 2;

[0064] 3. The esterified liquid material 2 of step 2 is introduced into nitrogen and pressed into a condensation reaction kettle. When heated to 270°C, it is stirred and the pressure is reduced to less than 1KPa. The temperature is controlled at 285°C. The reaction is carried out for 1.5 hours. The vacuum jet pump is turned on. The pressure in the kettle reaches 65Pa. The reaction time is 4.5 hours. The material is discharged, pelletized, and dried to obtain a copolyester material.

[0065] Example 2

[0066] A weather-resistant non-crystalline copolyester material comprises the following raw materials, measured by weight: 30 parts of terephthalic acid, 20 parts of ethylene glycol, 5 parts of neopentyl glycol, 10 parts of 1,4-cyclohexanedimethanol, 0.05 parts of supported catalyst A, 0.01 parts of trimethyl phosphate, 2 parts of amidine ultraviolet absorber A, and 10100.5 parts of antioxidant.

[0067] The preparation method of the copolyester material of this embodiment comprises the following steps:

[0068] 1. Put terephthalic acid, ethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol and supported catalyst A into a beating kettle for mixing and beating to prepare slurry, and beat for 30 minutes. Then, send them into esterification reaction kettle 1 through a screw slurry delivery pump for esterification at normal pressure. The temperature in the kettle is controlled at 235° C. to obtain esterification liquid 1;

[0069] 2. Nitrogen is introduced into the esterification reaction kettle 1, and the esterification liquid material 1 of step 1 is pressed into the esterification reaction kettle 2. The amidine ultraviolet absorber A and the antioxidant 1010 are mixed and put into the kettle together with trimethyl phosphate and stirred for 10 minutes. The temperature in the kettle is controlled at 220° C. to obtain the esterification liquid material 2;

[0070] 3. The esterified liquid material 2 of step 2 is introduced into nitrogen and pressed into a condensation reaction kettle. When heated to 260°C, it is stirred and the pressure is reduced to less than 1KPa. The temperature is controlled at 280°C. The reaction is carried out for 2h. The vacuum jet pump is turned on. The pressure in the kettle reaches 50Pa. The reaction time is 3.5h. The material is discharged, pelletized, and dried to obtain a copolyester material.

[0071] Example 3

[0072] A weather-resistant non-crystalline copolyester material comprises the following raw materials, measured by weight: 80 parts of terephthalic acid, 30 parts of ethylene glycol, 10 parts of neopentyl glycol, 20 parts of tricyclodecane dimethanol, 0.25 parts of supported catalyst A, 0.2 parts of trimethyl phosphate, 5 parts of amidine ultraviolet absorber A, and 10101 parts of antioxidant.

[0073] The preparation method of the copolyester material of this embodiment comprises the following steps:

[0074] 1. Put terephthalic acid, ethylene glycol, neopentyl glycol, 1,4-cyclohexanedimethanol and supported catalyst A into a beating kettle for mixing and beating to prepare slurry, and beat for 45 minutes. Then, send them into esterification reaction kettle 1 through a screw slurry delivery pump for normal pressure esterification. The temperature in the kettle is controlled at 250° C. to obtain esterification liquid 1;

[0075] 2. Nitrogen is introduced into the esterification reaction kettle 1, and the esterification liquid material 1 of step 1 is pressed into the esterification reaction kettle 2. The amidine ultraviolet absorber A and the antioxidant 1010 are mixed and put into the kettle together with trimethyl phosphate and stirred for 20 minutes. The temperature in the kettle is controlled at 260° C. to obtain the esterification liquid material 2;

[0076] 3. The esterified liquid material 2 of step 2 is introduced into nitrogen and pressed into a condensation reaction kettle. When heated to 280°C, it is stirred and the pressure is reduced to less than 1KPa. The temperature is controlled at 295°C. The reaction is carried out for 1 hour. The vacuum jet pump is turned on. The pressure in the kettle reaches 80Pa. The reaction time is 5 hours. The material is discharged, pelletized, and dried to obtain a copolyester material.

[0077] Example 4

[0078] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of supported catalyst B is used to replace supported catalyst A.

[0079] Example 5

[0080] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of supported catalyst C is used to replace supported catalyst A.

[0081] Example 6

[0082] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of an amidine ultraviolet absorber B is used to replace the amidine ultraviolet absorber A.

[0083] Example 7

[0084] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of an amidine ultraviolet absorber C is used to replace the amidine ultraviolet absorber A.

[0085] Comparative Example 1

[0086] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of neopentyl glycol is used to replace 1,4-cyclohexanedimethanol.

[0087] Comparative Example 2

[0088] A weather-resistant non-crystalline copolyester material and a preparation method thereof. The specific implementation manner is the same as that of Example 1, except that an equal amount of commercially available ultraviolet absorber UV-326 is used to replace the amidine ultraviolet absorber A.

[0089] Effect evaluation:

[0090] The copolyester materials prepared in the above Examples 1-7 and Comparative Examples 1-2 were tested and analyzed, and the specific results are shown in Table 1.

[0091] Performance Test:

[0092] (1) Mechanical properties: According to GB / T 1040.2-2022 Determination of tensile properties of plastics, the tensile properties test and elongation at break test were carried out using a CMT6104 universal testing machine at a tensile speed of 50 mm / min.

[0093] (2) Weathering test: Light source exposure test was carried out according to standard GB / T16422.3-2022, using method A: UVA-340 lamp at 340nm 0.76W / (m 2·nm), blackboard temperature 60±3℃, tensile strength of copolyester material after 60h test with fluorescent UV lamp. Ultraviolet radiation is the main factor affecting the weather resistance of copolyester material, and its weather resistance is reflected by the tensile strength after radiation.

[0094] Table 1

[0095] Serial number Tensile strength / MPa Elongation at break / % Tensile strength after weathering / MPa Example 1 17.1 1122 16.2 Example 2 16.0 1089 15.0 Example 3 16.6 1105 15.7 Example 4 15.9 1002 14.9 Example 5 14.3 881 13.4 Example 6 16.1 1043 13.0 Example 7 15.8 967 12.2 Comparative Example 1 13.9 784 11.5 Comparative Example 2 16.5 1095 10.4

[0096] It can be seen from Table 1 that the copolyester materials prepared in Examples 1-3 have excellent weather resistance and good mechanical properties.

[0097] Compared with Example 1, when preparing the supported catalyst, the mass ratio of graphene oxide and 1-aminoethyl-3-methylimidazolium tetrafluoroborate was changed, the imidazole ring amount was reduced, the stacking and overlapping of graphene oxide was caused, and the specific surface area of ​​graphene oxide was reduced, which affected the catalytic performance and further affected the performance of the finally synthesized copolyester material.

[0098] Compared with Example 1, when preparing the supported catalyst, Example 5 changes the mass ratio of the reducing agent to graphene oxide, which weakens the reducing property, is not conducive to forming a stable catalyst, affects the catalytic activity, and further affects the performance of the finally synthesized copolyester material.

[0099] Compared with Example 1, Example 6 changes the organic solvent when preparing the amidine ultraviolet absorber, resulting in incomplete dissolution and dispersion of the raw materials, and thus the synthesized ultraviolet absorber has poor performance and affects weather resistance.

[0100] Compared with Example 1, in Example 7, the molar ratio of N,N'-bis(4-ethoxycarbonylphenyl)formamidine and 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene is changed when preparing the amidine ultraviolet absorber, so that the amidine ultraviolet absorber does not have a symmetrical structure, the conjugation effect is weakened, the absorption capacity of ultraviolet light becomes worse, and the weather resistance is affected.

[0101] Compared with Example 1, Comparative Example 1 does not add alicyclic diol, which will make the material closer to the crystalline direction, the overall performance is uneven, and the weather resistance and mechanical properties are affected.

[0102] In Comparative Example 2, compared with Example 1, an equal amount of commercially available ultraviolet absorber UV-326 was used to replace the amidine ultraviolet absorber A. The ultraviolet absorber had poor performance and affected the weather resistance.

[0103] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.

Claims

1. A weather-resistant non-crystalline copolyester material, characterized in that: The raw materials include the following by weight: 30-80 parts of terephthalic acid, 20-30 parts of ethylene glycol, 5-10 parts of neopentyl glycol, 10-20 parts of alicyclic diol, 0.05-0.25 parts of supported catalyst, 0.01-0.2 parts of stabilizer, 2-5 parts of amidine ultraviolet absorber and 0.5-1 parts of antioxidant.

2. The weather-resistant non-crystalline copolyester material according to claim 1, characterized in that: The method for preparing the supported catalyst comprises the following steps: S1. Graphene oxide is dispersed in deionized water, 1-aminoethyl-3-methylimidazolium tetrafluoroborate is added, the mixture is poured into a reaction kettle, potassium hydroxide is added, and ultrasonic treatment is performed for 30-45 minutes to obtain a mixture containing an ionic liquid; S2. The mixture containing the ionic liquid obtained in step S1, antimony glycol and tetrabutoxygermanium were added to the reactor, ultrasonically treated for 30-45 min, and stirred for 12-16 h to obtain a mixed solution; S3. Add a reducing agent to the mixed solution obtained in step S2, stir for 20-30 minutes, dry at 80-90° C. for 5-6 hours, cool to room temperature, wash, and obtain a supported catalyst.

3. The weather-resistant non-crystalline copolyester material according to claim 2, characterized in that: The mass ratio of graphene oxide to 1-aminoethyl-3-methylimidazolium tetrafluoroborate in step S1 is (0.5-0.8):

1.

4. The weather-resistant non-crystalline copolyester material according to claim 2, characterized in that: The mass ratio of the reducing agent in step S3 to the graphene oxide in step S1 is (2.5-3):

1.

5. The weather-resistant non-crystalline copolyester material according to claim 1, characterized in that: The preparation method of the amidine ultraviolet absorber comprises the following steps: Add N,N'-bis(4-ethoxycarbonylphenyl)formamidine and a composite organic solvent into a reaction kettle, stir to dissolve, add potassium carbonate under an inert gas protection atmosphere, heat to 60-80°C, keep warm for 0.5-1.5h, add 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene, heat to 90-120°C, keep warm for 2-5h, cool, rotary evaporate, and recrystallize to obtain a novel amidine ultraviolet absorber.

6. The weather-resistant non-crystalline copolyester material according to claim 5, characterized in that: The composite organic solvent is N,N-dimethylformamide and acetonitrile, and the volume ratio of the two is 1:(1.5-3).

7. The weather-resistant non-crystalline copolyester material according to claim 5, characterized in that: The molar ratio of the N,N'-bis(4-ethoxycarbonylphenyl)formamidine to 2,3,5,6-tetrafluoro-1,4-bis(chloromethyl)benzene is (2-2.5):

1.

8. The weather-resistant non-crystalline copolyester material according to claim 1, characterized in that: The antioxidant is any one or more of hindered phenols, hindered amines and phosphites.

9. The weather-resistant non-crystalline copolyester material according to claim 1, characterized in that: The alicyclic diol is any one or more of 1,4-cyclohexanedimethanol, tricyclodecane dimethanol and bicyclo[2.2.1]heptane-2,2-dimethanol.

10. A method for preparing the weather-resistant non-crystalline copolyester material according to any one of claims 1 to 9, characterized in that: The following steps are included:

1. Put terephthalic acid, ethylene glycol, neopentyl glycol, alicyclic diol and supported catalyst into a beating kettle for mixing and beating to prepare slurry, and beat for 30-45 minutes, and then put it into an esterification reaction kettle 1 for esterification at normal pressure, and control the temperature in the kettle at 230-280° C. to obtain esterification liquid 1; 2. Introduce inert gas into the esterification reaction kettle 1, pressurize the esterification liquid material 1 of step 1 into the esterification reaction kettle 2, mix the amidine ultraviolet absorber and antioxidant and put them into the kettle together with the stabilizer and stir for 10-20 minutes, and control the temperature in the kettle at 220-260° C. to obtain the esterification liquid material 2; 3. The esterified liquid material 2 of step 2 is introduced into an inert gas and pressed into a polycondensation reaction kettle. When heated to 260-280°C, the pressure is pumped down to less than 1KPa by stirring. The temperature is controlled at 280-295°C. The reaction is carried out for 1-2h. The vacuum jet pump is turned on. The pressure in the kettle reaches 50-80Pa. The reaction time is 3.5-5h. The material is discharged, pelletized and dried to obtain a copolyester material.