PLA-based adhesive tape
By using self-made plasticizers and functional additives, combined with biaxial stretching process, PLA-based tapes were prepared, solving the problems of poor mechanical properties and poor bonding strength in humid environments, and realizing the application of high-performance biodegradable tapes.
Patent Information
- Application Number
- CN202410982567.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-11-12
AI Technical Summary
Existing biodegradable tapes have poor mechanical properties and poor adhesion strength in humid environments. Furthermore, the materials are not easy to separate and recycle, leading to white pollution problems.
Using PLA as the base material, and through self-made plasticizers, plant oil-based resins, and hyperbranched lactic acrylate and other functional additives, combined with biaxial stretching process, a three-layer structure tape is prepared to enhance the toughness of the base material and the compatibility of the adhesive layer, thereby improving the bonding strength.
This technology enables PLA-based tapes to maintain high bonding strength in humid environments, and the material is biodegradable, solving the problem of white pollution and improving the overall performance of the tapes.
Smart Images

Figure BDA0004956510440000191 
Figure BDA0004956510440000201
Abstract
Description
Technical Field
[0001] The invention relates to a PLA-based adhesive tape and a preparation method thereof. The invention belongs to the field of degradable films. Background Art
[0002] At present, the express delivery industry uses a large number of sealing tapes. The base film materials of the tapes are mostly BOPP or PVC, and the adhesives are mostly acrylic or ethylene-vinyl acetate copolymer adhesives. They have excellent performance and pressure-sensitive adhesive properties. However, both the base film materials and adhesive materials are synthetic non-degradable materials. During their large-scale use, they are not easy to separate from the cartons, making it difficult to recycle the cartons. At the same time, non-degradable materials are prone to white pollution, which has become a serious social problem. Based on this, people have proposed a variety of solutions, among which the fundamental solution is to replace existing packaging materials with degradable and recyclable materials.
[0003] Polylactic acid (PLA) is a new type of degradable polymer material with biomass origin and degradable properties. It is suitable for disposable and short-term use products and is the only transparent biodegradable polymer. The biaxial stretching method can be used to prepare high-strength and high-transparency film products, which can be used as the tape substrate to prepare new degradable tapes.
[0004] PLA has high mechanical strength. The tensile strength of its biaxially stretched film can reach more than 120MPa. Even without stretching orientation, its tensile strength reaches about 70MPa. It seems to be a feasible solution to prepare a series of flexible tapes by preparing a blended film with PLA as the substrate to adjust the mechanical strength of the film. However, the following problems still need to be solved: first, the toughening modification of PLA. Due to the easy crystallization of PLA, it is brittle and difficult to form a film directly alone; second, the compatibility of PLA with existing adhesives is too good or too poor, which is not conducive to the preparation of high-performance tapes. If the compatibility is too good, the tape is easy to stick together after being rolled, affecting the use effect. If the compatibility is too poor, it is easy to peel off and affect the bonding strength; and both the substrate and the adhesive layer must have degradable properties; finally, the bonding strength of most existing tapes in humid environments is poor.
[0005] In view of the above-mentioned problems of the degradable material PLA, it is of great significance to modify the PLA substrate, improve its processability and toughness, and modify the adhesive layer on the PLA-based tape. Summary of the invention
[0006] The purpose of the present invention is to provide a method for preparing a PLA-based tape in view of the defects of poor mechanical properties and poor bonding strength in a humid environment in the degradable tape in the prior art. The plasticizer applied to the substrate, the plant oil-based resin applied to the adhesive layer and the functional additive are prepared by molecular structure design, and the substrate is extruded and biaxially stretched after formula design, and then the release layer and the adhesive layer are coated on both sides. The technical solution adopted by the present invention to solve its technical problems is:
[0007] The present invention provides a method for preparing a plasticizer, comprising the following steps:
[0008] S11, performing silylation coupling reaction on nano-silicon and epoxy silane coupling agent to obtain intermediate product 1I;
[0009] S12, subjecting the intermediate product 1I to esterification and ring-opening reaction with lactic acid to obtain the target product, i.e., the plasticizer.
[0010] Furthermore, the usage ratio of the nano silicon to the epoxy silane coupling agent is 1g:5.0-7.0g.
[0011] Furthermore, the intermediate product II and lactic acid are added at a molar ratio of epoxy group to carboxyl group of 1:5-10.
[0012] The present invention provides a plasticizer prepared by the above-mentioned plasticizer preparation method.
[0013] Another object of the present invention is to provide a method for preparing a vegetable oil-based resin, comprising the following steps:
[0014] S21, click reaction of vegetable oil with thiol derivatives to obtain intermediate 2I;
[0015] S22, coupling reaction of the intermediate product 2I with the acryloyl structure A to obtain the target product, i.e., the plant oil-based resin.
[0016] Furthermore, the vegetable oil and the thiol derivative are added in a molar ratio of 1:3-5; and
[0017] The vegetable oil is a drying oil or a semi-drying oil.
[0018] Further,
[0019] The intermediate product 2I and the acryloyl structure A are mixed in a molar ratio of 1:1 based on the reaction functional groups; and
[0020] The acryl structure A contains a functional group that can react with the hydroxyl structure.
[0021] Another object of the present invention is to provide a plant oil-based resin prepared by the above-mentioned method for preparing the plant oil-based resin.
[0022] Another object of the present invention is to provide a method for preparing hyperbranched lactic acid acrylate, comprising the following steps:
[0023] S31, coupling reaction of the plasticizer with the acryloyl structure B to obtain the target product, namely, hyperbranched lactic acid acrylate.
[0024] Furthermore, the plasticizer and the acryl structure B are added at a molar ratio of hydroxyl group to acryl structure B of 2.0-10.0:1; and
[0025] The acryl structure B contains a functional group that can react with the hydroxyl structure.
[0026] Another object of the present invention is to provide a hyperbranched lactic acid acrylate prepared by the preparation method of the functional monomer.
[0027] Another object of the present invention is to provide a method for preparing a functional monomer, comprising the following steps:
[0028] S41, subjecting catechin to a ring-opening reaction with glycidyl methacrylate to obtain a target product, namely a functional monomer.
[0029] Furthermore, the catechin and glycidyl methacrylate are added in a molar ratio of 1:1.
[0030] Another object of the present invention is to provide a functional monomer prepared by the above-mentioned method for preparing the functional monomer.
[0031] Another object of the present invention is to provide a PLA-based tape, comprising a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively;
[0032] The substrate comprises the following raw materials in parts by weight:
[0033] PLA 60-80 parts;
[0034] PBAT 20-40 parts;
[0035] Compatibilizer 0.5-1.0 part;
[0036] Plasticizer 5.0-10.0 parts;
[0037] Antioxidant 0.3-0.5 parts;
[0038] Lubricant 0.5-1.0 part;
[0039] Among them, the total mass of PLA and PBAT is 100 parts;
[0040] The adhesive layer comprises the following raw materials in percentage by weight:
[0041] Hyperbranched lactic acid acrylate 35-45 parts;
[0042] 25-35 parts of vegetable oil-based resin;
[0043] 2.0-3.0 parts of functional monomer;
[0044] 5-10 parts of diluent;
[0045] Photoinitiator 2.0-4.0 parts;
[0046] Defoaming agent 0.1-0.2 parts;
[0047] Leveling agent 0.1-0.3 parts;
[0048] Solvent Residue.
[0049] The present invention also provides a method for preparing a PLA-based adhesive tape, comprising the following steps:
[0050] S51, preparation of substrate, i.e.
[0051] The raw materials are mixed evenly according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film;
[0052] S52, coating a release layer, i.e.
[0053] Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling; and
[0054] S53, the other side of the substrate is coated with an adhesive layer, i.e.
[0055] The adhesive layer solution is prepared according to the ratio, and after adjusting the online viscosity, it is coated on the substrate by gravure, put into the drying tunnel, and the drying temperature is controlled at 45-80℃. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape is obtained.
[0056] Beneficial effects of the present invention:
[0057] (1) The present invention provides a PLA-based adhesive tape, wherein the base material formula contains a self-made plasticizer, which is a hyperbranched structure with nano-silicon as the core, lactic acid oligomer as the chain structure and hydroxyl as the terminal group. First, lactic acid oligomer is an excellent plasticizer for PLA, which can effectively improve the processing performance and mechanical properties; second, the hyperbranched structure has good fluidity, which can further improve the plasticization efficiency and is not easy to migrate and precipitate.
[0058] (2) The present invention provides a PLA-based adhesive tape, wherein the adhesive layer formula raw material contains self-made hyperbranched lactic acid acrylate, which is a hyperbranched nano-silicon microsphere structure of acrylate-terminated lactic acid oligomers. First, the lactic acid oligomer structure is conducive to improving the compatibility between the adhesive layer and the substrate; second, the hyperbranched microsphere structure has multiple functionalities and isotropy, which can improve the cohesion and adhesion of the adhesive layer; third, a large number of terminal hydroxyl groups remain in the microsphere structure, which can further improve the bonding performance.
[0059] (3) The present invention provides a PLA-based adhesive tape, wherein the adhesive layer formula raw material contains a self-made plant oil-based resin, which is a plant oil-based acrylate structure. First, the acryloxy structure has excellent compatibility with hyperbranched lactic acid acrylate; second, the plant oil structure is a flexible chain, which has the function of releasing internal stress and can improve adhesion, etc.
[0060] (4) The present invention provides a PLA-based adhesive tape, wherein the adhesive layer formula raw material contains a self-made functional monomer, which is a catechin acrylate structure. Catechol has an excellent bonding effect, especially in a humid environment, and can promote the effective bonding of the adhesive layer to various objects.
[0061] (5) The present invention provides a PLA-based adhesive tape, wherein the base material portion is mainly composed of PLA and PBAT is blended for toughening and modification, which can provide better mechanical strength and toughness, and both PLA and PBAT are degradable materials; the adhesive layer portion is mainly composed of lactic acid acrylate and vegetable oil-based resin, which can improve adhesion, and lactic acid oligomers and vegetable oil are both degradable materials, and has practical application potential. DETAILED DESCRIPTION
[0062] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0063] The purpose of the present invention is to develop a new type of PLA-based adhesive tape. The design idea is: design a three-layer structure with PLA as the main body, an adhesive layer coated on one side, and a release layer coated on the other side; and both the substrate and the adhesive layer are degradable materials. The problems faced are: 1. The toughening problem of the PLA-based substrate; 2. The problem of the bonding strength of the adhesive layer. Solution: First, the toughening problem of PLA, PLA and PBAT are blended and modified, and a commonly used commercially available compatible chain extender is added, and a plasticizer with a hyperbranched structure containing lactic acid oligomers is made to improve the flexibility of the substrate without precipitation. Second, the main raw materials in the homemade adhesive layer include main resin and functional monomer; one of the main resins is a hyperbranched lactic acid oligomer acrylate structure, which provides isotropic cohesion of the adhesive layer to improve the bonding strength and has excellent compatibility with the substrate; the plant oil-based acrylate of one of the main resins provides flexibility of the adhesive layer, releases internal stress, and improves bonding strength; the functional monomer is an acrylate containing a catechol structure, and the catechol structure has excellent bonding strength and water resistance, and still has high bonding performance even in a humid environment. And the above components are all degradable components. The theoretical basis for the realization is: first, the homemade plasticizer uses nano-silicon and epoxy silane coupling agent for coupling reaction, and the carboxyl group in the lactic acid oligomer formed by self-polymerization and epoxy are subjected to a ring-opening reaction to prepare a hyperbranched plasticizer containing a hydroxyl-terminated lactic acid oligomer structure connection. Second, the homemade hyperbranched lactic acid oligomer acrylate structure, on the basis of the plasticizer, the hydroxyl group is substituted to obtain a product containing an acrylate structure. Third, the homemade plant oil-based resin, the plant oil and thiol are subjected to a click addition reaction to prepare a structure containing a hydroxyl or carboxyl group at the end group; and then the product is prepared by a substitution reaction with an acryloyl group. Fourth, the homemade functional monomer is prepared by a ring-opening addition reaction of catechin and glycidyl methacrylate. Finally, after formula design and taking into account the role of each polar group of the monomer diluent in the adhesive layer, an adhesive layer solution is prepared, and it is coated on a substrate treated with a biaxial stretching process to obtain a PLA-based tape material with effectively improved properties including mechanical properties and bonding strength. The components work synergistically with each other to effectively improve the comprehensive performance, etc. The embodiments of the present invention are as follows:
[0064] The embodiment of the present invention provides a method for preparing a plasticizer, comprising the following steps:
[0065] S11, placing nano-silicon in ethyl acetate A, ultrasonically dispersing for 1 hour, adding epoxy silane coupling agent and deionized water A, slowly heating to 60-80°C, heating and stirring for 6-14 hours, after the reaction is completed, cooling to room temperature, filtering, washing with ethyl acetate B, and vacuum drying at 40°C to constant weight to obtain the target product, i.e., intermediate product 1I;
[0066] The dosage ratio of the nano silicon, ethyl acetate A, epoxy silane coupling agent, deionized water A, and ethyl acetate B is: 1.00 g: 50 mL: 5.0-7.0 g: 0.6 g: 200 mL.
[0067] The nano-silicon has an average particle size of 50-100 nm and is purchased from Ningbo Jinlei Nanomaterial Technology Co., Ltd.
[0068] The epoxy silane coupling agent may be silane coupling agent KH560, silane coupling agent A1871, etc., and preferably silane coupling agent KH560.
[0069] S12, under nitrogen protection, add lactic acid and catalyst into the reactor, heat to 155-165℃ for reaction for 2h, continue to heat to 175-185℃ for reaction for 2-4h, and observe the water quality; cool to 120-140℃, add intermediate product 1I, stir for 6-8h, cool to room temperature, distill under reduced pressure, and vacuum dry at 60℃ for 6h to obtain the target product, i.e. plasticizer.
[0070] The intermediate product II and lactic acid are added in a molar ratio of epoxy group to carboxyl group of 1:5-10.
[0071] The amount of the catalyst used is 0.4% of the total mass of the reactants;
[0072] The catalyst is a mixture of stannous octoate and p-toluenesulfonic acid in a mass ratio of 2:1; and the following embodiments all use the catalyst.
[0073] Since the polymerization of lactic acid is a dehydration condensation reaction, the molecular weight and degree of polymerization of PLA can be rationally controlled by the molar number of lactic acid added and the mass of separated water.
[0074] The embodiment of the present invention provides a method for preparing a plant oil-based resin, comprising the following steps:
[0075] S21, adding vegetable oil, thiol derivatives, and photoinitiator 184 to dichloromethane A, reacting under UV radiation at room temperature for 0.5-2h, washing with deionized water B three times, separating the liquids, taking the organic phase, drying with anhydrous sodium sulfate A, filtering, taking the filtrate, distilling under reduced pressure, and vacuum drying at 40°C for 12h to obtain the intermediate product 2I;
[0076] The vegetable oil, thiol derivative, dichloromethane A, deionized water B, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 3.0-5.0 mmol: 20 mL: 25 mL: 5 g;
[0077] The vegetable oil is a drying oil or a semi-drying oil.
[0078] The drying oil can be linseed oil, tung oil, etc.
[0079] The semi-drying oil can be rice bran oil, corn germ oil, soybean oil, safflower seed oil, sunflower seed oil, sesame oil, etc.
[0080] The thiol derivative may be a hydroxythiol or a carboxylthiol.
[0081] The hydroxythiol may be mercaptoethanol, 3-mercapto-1-propanol, 1-thioglycerol, etc., and mercaptoethanol is preferred.
[0082] The carboxyl mercaptan may be thiolactic acid, thioglycolic acid, 3-mercaptopropionic acid, 11-mercaptoundecanoic acid, etc., and preferably 3-mercaptopropionic acid.
[0083] The amount of the photoinitiator 184 is 2.0-4.0% of the total mass of the reactants;
[0084] The radiation energy intensity of the UV radiation device can be 300-500 mW / cm 2 ; Specifically, it can be 300mW / cm 2 、350mW / cm 2 , 400mW / cm 2 、450mW / cm 2 , 500mW / cm 2 , or a range of any two values; and the radiation energy intensity of the UV device described in the following embodiments of the present invention is 400mW / cm 2 .
[0085] S22, after mixing the intermediate product 2I and the acryloyl structure A, stirring at a set temperature for a period of time, distilling under reduced pressure, and vacuum drying at 40° C. for 12 hours to obtain the target product, namely, the plant oil-based resin.
[0086] The intermediate product 2I and the acryloyl structure A are mixed in a molar ratio of 1:1 based on the reaction functional groups;
[0087] The acryloyl structure A contains a functional group that can react with the hydroxyl structure; and the acryloyl structure A can be isocyanoethyl methacrylate, acryloyl chloride, glycidyl methacrylate, etc.;
[0088] The structure of the acryloyl structure A is adjusted according to the thiol structure; specifically, if the thiol structure is hydroxy thiol, the acryloyl structure A can be isocyanoethyl methacrylate, acryloyl chloride, glycidyl methacrylate, etc.; if the thiol structure is carboxyl thiol, the acryloyl structure A can be glycidyl methacrylate, etc.
[0089] The embodiment of the present invention provides a method for preparing hyperbranched lactic acid acrylate, comprising the following steps:
[0090] S31, adding a plasticizer and an acryloyl structure B to dichloromethane C, stirring at 50-80° C. for 6-10 h, distilling under reduced pressure, and vacuum drying at 40° C. for 12 h to obtain the target product, i.e., hyperbranched lactic acid acrylate.
[0091] The plasticizer and the acryl structure B are added at a molar ratio of hydroxyl group to acryl structure B of 2.0-10.0:1;
[0092] The usage ratio of the plasticizer to dichloromethane C is 1 g: 20 mL;
[0093] The acryloyl structure B contains a functional group that can react with the hydroxyl structure; the acryloyl structure B can be isocyanoethyl methacrylate, acryloyl chloride, glycidyl methacrylate, etc., and isocyanoethyl methacrylate is preferred.
[0094] In the present invention, the acryl structure B and the acryl structure A may be the same as or different from each other.
[0095] The embodiment of the present invention provides a method for preparing a functional monomer, comprising the following steps:
[0096] S41, add catechin, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water C, shake, add ethyl acetate C for extraction, take the organic phase, dry it with anhydrous sodium sulfate B, filter, take the filtrate, distill it under reduced pressure, and vacuum dry it at 40°C for 12 hours to obtain the target product, i.e., the functional monomer.
[0097] The catechin, glycidyl methacrylate, tetrabutylammonium bromide, tetrahydrofuran, deionized water C, ethyl acetate C, and anhydrous sodium sulfate B are added in a ratio of 1 mmol: 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g;
[0098] The amount of hydroquinone used is 0.1wt% of the mass of glycidyl methacrylate.
[0099] The catechin may be protocatechuic acid or plateau catechuic acid; and, preferably, protocatechuic acid.
[0100] Another object of the present invention is to provide a PLA-based tape, comprising a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively;
[0101] The substrate comprises the following raw materials in parts by weight:
[0102] PLA 60-80 parts;
[0103] PBAT 20-40 parts;
[0104] Compatibilizer 0.5-1.0 part;
[0105] Plasticizer 5.0-10.0 parts;
[0106] Antioxidant 0.3-0.5 parts;
[0107] Lubricant 0.5-1.0 part;
[0108] Among them, the total mass of PLA and PBAT is 100 parts;
[0109] The melt index of the PLA is 2.5-3.5 g / 10 min (190° C., 2.16 kg); the model of the PLA described in the following embodiments of the present invention is PT102, purchased from Pulisi Biotechnology Co., Ltd. PT102 PLA has self-nucleation ability and can crystallize quickly.
[0110] The brand of PBAT described in the following embodiments of the present invention is TH801T, which was purchased from Xinjiang Blue Mountain Tunhe Polyester Co., Ltd.
[0111] The compatibilizer described in the following examples of the present invention is Joncryl ADR 4368, produced by BASF.
[0112] The antioxidant is a hindered phenol; it can be antioxidant 1010, antioxidant 1076, antioxidant 264, antioxidant 2246, etc.; and the antioxidant described in the following embodiments of the present invention is antioxidant 1010.
[0113] The lubricant may be erucamide, oleamide, ethylene bisstearamide, etc.; and, the lubricant described in the following embodiments of the present invention is erucamide and ethylene bisstearamide mixed and added in a mass ratio of 2 / 1.
[0114] The adhesive layer comprises the following raw materials in percentage by weight:
[0115] Hyperbranched lactic acid acrylate 35-45 parts;
[0116] 25-35 parts of vegetable oil-based resin;
[0117] 2.0-3.0 parts of functional monomer;
[0118] 5-10 parts of diluent;
[0119] Photoinitiator 2.0-4.0 parts;
[0120] Defoaming agent 0.1-0.2 parts;
[0121] Leveling agent 0.1-0.3 parts;
[0122] Solvent Residue.
[0123] The diluent can be (meth)acrylic acid, methyl (meth)acrylate, ethyl (meth)acrylate, butyl acrylate, isobutyl acrylate, tert-butyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, isooctyl acrylate, decyl acrylate, 2-ethoxyethyl acrylate, cyclohexyl acrylate, glycidyl methacrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, etc.
[0124] The photoinitiator can be photoinitiator 184, photoinitiator 1173, photoinitiator 2959, photoinitiator TPO, etc.
[0125] The defoaming agent described in the following examples of the present invention is Digo 920.
[0126] The leveling agent described in the following examples of the present invention is BYK333.
[0127] The solvent described in the following examples of the present invention is a mixture of butanone and ethyl acetate in a mass ratio of 2:1.
[0128] The solvent in the present invention has good solubility for PLA. When the adhesive layer solution is coated on the surface of the substrate, slight swelling will occur, which promotes the adhesion between the substrate and the adhesive layer and avoids the process of corona treatment of the substrate.
[0129] The release layer described in the following embodiments of the present invention comprises the following raw materials in parts by weight:
[0130] Vinyl dimethicone 90 parts;
[0131] 4 parts of methyl hydrogen polysiloxane;
[0132] 1 part of chloroplatinic acid-isopropanol catalyst;
[0133] 0.6 parts of 3-glycidyloxypropyltriethoxysilane;
[0134] 0.1 part of methylbutynol;
[0135] 300 parts of solvent: toluene.
[0136] The present invention also provides a method for preparing a PLA-based adhesive tape, comprising the following steps:
[0137] S51, preparation of substrate, i.e.
[0138] The raw materials are mixed evenly according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film (thickness 45-55 μm);
[0139] The twin-screw extruder is set with the temperature of each zone at 150-190°C, the die head temperature at 190-200°C, and the casting temperature at 30-50°C.
[0140] The biaxial stretching parameters are: stretching ratio of 3.0-4.0; temperature of 70-90°C; speed of 60-100 mm / s;
[0141] The heat setting is performed at 90-100° C. for 10-20 minutes.
[0142] S52, coating a release layer, i.e.
[0143] Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling (release layer thickness 1-3μm); and
[0144] S53, the other side of the substrate is coated with an adhesive layer, i.e.
[0145] The adhesive layer solution is prepared according to the ratio, and after adjusting the online viscosity, it is coated on the substrate by gravure, put into the drying tunnel, and the drying temperature is controlled at 45-80℃. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape is obtained.
[0146] The UV curing radiation energy is 400 mJ / cm 2 ; The thickness of the adhesive layer is 10-15μm.
[0147] In order to further understand the present invention, a PLA-based adhesive tape provided by the present invention is described in detail below in conjunction with specific embodiments, and the protection scope of the present invention is not limited by the following embodiments.
[0148] Example 1
[0149] A method for preparing a plasticizer comprises the following steps:
[0150] S11, placing nano-silicon in ethyl acetate A, ultrasonically dispersing for 1 hour, adding epoxy silane coupling agent KH560 and deionized water A, slowly heating to 70°C, heating and stirring for 10 hours, after the reaction is completed, cooling to room temperature, filtering, washing with ethyl acetate B, and vacuum drying at 40°C to constant weight to obtain the target product, i.e., intermediate product 1I;
[0151] The dosage ratio of the nano-silicon, ethyl acetate A, epoxy silane coupling agent, deionized water A, and ethyl acetate B is: 1.00 g: 50 mL: 6.0 g: 0.6 g: 200 mL.
[0152] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1265cm -1 、938cm-1 、801cm -1 : Epoxy group exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0153] S12, under nitrogen protection, lactic acid and catalyst are added to the reactor, the temperature is raised to 160°C for reaction for 2h, the temperature is further raised to 180°C for reaction for 2.5h, and the water separation quality is observed; the temperature is lowered to 130°C, the intermediate product 1I is added, stirred for 6.5h, cooled to room temperature, distilled under reduced pressure, and vacuum dried at 60°C for 6h to obtain the target product, i.e., plasticizer (average degree of polymerization is 7.8).
[0154] The intermediate product 1I and lactic acid are added at a molar ratio of epoxy group to carboxyl group of 1:8.
[0155] The amount of the catalyst used is 0.4% of the total mass of the reactants.
[0156] Its infrared data are as follows: 3382cm -1 :-OH exists and is significantly enhanced; 1735cm -1 :-C=O exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group does not exist; 1109cm -1 、801cm -1 :-Si-O- exists.
[0157] A method for preparing a vegetable oil-based resin comprises the following steps:
[0158] S21, soybean oil, mercaptoethanol, and photoinitiator 184 were added to dichloromethane A, and the reaction was carried out under UV radiation at room temperature for 0.5 h, and the mixture was washed with deionized water B three times, and the organic phase was separated, dried with anhydrous sodium sulfate A, filtered, and the filtrate was distilled under reduced pressure and dried in vacuo at 40°C for 12 h to obtain the intermediate product 2I;
[0159] The soybean oil, mercaptoethanol, dichloromethane A, deionized water B, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 4.0 mmol: 20 mL: 25 mL: 5 g;
[0160] The amount of the photoinitiator 184 used is 4.0% of the total mass of the reactants.
[0161] Its infrared data are as follows: 3381cm -1 :-OH exists; 2550cm -1 :-SH does not exist; 1621cm -1 :-C=C- does not exist.
[0162] S22, add the intermediate product 2I, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone to dichloromethane B, stir at 80°C for 6 hours, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., plant oil-based resin.
[0163] The intermediate product 2I and the acryloyl structure A are mixed in a molar ratio of 1:1 based on the reaction functional groups;
[0164] The ratio of the intermediate product 2I to dichloromethane B is 1 mmol:20 mL;
[0165] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0166] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0167] Its infrared data are as follows: 3381cm -1 :-OH does not exist; 2270cm -1 :-NCO does not exist; 1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists.
[0168] A method for preparing hyperbranched lactic acid acrylate comprises the following steps:
[0169] S31, adding plasticizer, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone into dichloromethane C, stirring at 60° C. for 8 h, distilling under reduced pressure, and vacuum drying at 40° C. for 12 h to obtain the target product, i.e., hyperbranched lactic acid acrylate.
[0170] The plasticizer and isocyanoethyl methacrylate are added at a molar ratio of hydroxyl group to isocyanoethyl methacrylate of 7.0:1;
[0171] The usage ratio of the plasticizer to dichloromethane C is 1 g:20 mL.
[0172] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0173] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0174] Its infrared data are as follows: 3382cm -1 :-OH exists and weakens; 1735cm -1 、1680cm-1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0175] A method for preparing a functional monomer comprises the following steps:
[0176] S41, add protocatechuic acid, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat and reflux for 24 hours, cool to room temperature, add deionized water C, shake, add ethyl acetate C for extraction, take the organic phase, dry it with anhydrous sodium sulfate B, filter, take the filtrate, distill it under reduced pressure, and vacuum dry it at 40°C for 12 hours to obtain the target product, i.e., the functional monomer.
[0177] The protocatechuic acid, glycidyl methacrylate, tetrabutylammonium bromide, tetrahydrofuran, deionized water C, ethyl acetate C, and anhydrous sodium sulfate B are added in a ratio of 1 mmol: 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g;
[0178] The amount of hydroquinone used is 0.1wt% of the mass of glycidyl methacrylate.
[0179] Its infrared data are as follows: 3421cm -1 :-OH exists; 1760cm -1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group does not exist.
[0180] A PLA-based tape comprises a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively;
[0181] The substrate comprises the following raw materials in parts by weight:
[0182] PLA 70 parts;
[0183] PBAT 30 copies;
[0184] Compatibilizer 0.8 parts;
[0185] 8.0 parts of plasticizer;
[0186] 0.4 parts of antioxidant;
[0187] 0.7 parts of lubricant;
[0188] The adhesive layer comprises the following raw materials in percentage by weight:
[0189] 40 parts of hyperbranched lactic acid acrylate;
[0190] 30 parts of vegetable oil-based resin;
[0191] 2.5 parts of functional monomer;
[0192] 2 parts of methacrylic acid;
[0193] 2 parts of 2-ethylhexyl acrylate;
[0194] 1 part of glycidyl methacrylate;
[0195] 2 parts of hydroxyethyl methacrylate;
[0196] Photoinitiator 184 3.0 parts;
[0197] Defoaming agent 0.1 part;
[0198] 0.2 parts of leveling agent;
[0199] Solvent Residue.
[0200] A method for preparing a PLA-based adhesive tape comprises the following steps:
[0201] S51, preparation of substrate, i.e.
[0202] The raw materials are uniformly blended according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film (thickness of 50 μm);
[0203] The twin-screw extruder is set with the temperature of zone 1 at 160°C, zone 2 at 170°C, zone 3 at 180°C, zone 4 at 190°C, die head temperature at 195°C, and casting temperature at 40°C.
[0204] The biaxial stretching parameters are: stretching ratio of 3.5; temperature of 80° C.; and speed of 80 mm / s.
[0205] The heat setting is performed at 95° C. for 15 minutes.
[0206] S52, coating a release layer, i.e.
[0207] Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling (the release layer thickness is 2 μm); and
[0208] S53, the other side of the substrate is coated with an adhesive layer, i.e.
[0209] The adhesive layer solution was prepared according to the ratio, and after adjusting the online viscosity, it was coated on the substrate by gravure, put into the drying tunnel, and the drying temperature was controlled at 70°C. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape (adhesive layer thickness 14 μm) was obtained.
[0210] Example 2
[0211] The rest is the same as in Example 1, except that:
[0212] A method for preparing a plasticizer comprises the following steps:
[0213] S11, placing nano-silicon in ethyl acetate A, ultrasonically dispersing for 1 hour, adding epoxy silane coupling agent KH560 and deionized water A, slowly heating to 60°C, heating and stirring for 14 hours, after the reaction is completed, cooling to room temperature, filtering, washing with ethyl acetate B, and vacuum drying at 40°C to constant weight to obtain the target product, i.e., intermediate product 1I;
[0214] The dosage ratio of the nano silicon, ethyl acetate A, epoxy silane coupling agent, deionized water A, and ethyl acetate B is: 1.00 g: 50 mL: 7.0 g: 0.6 g: 200 mL.
[0215] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0216] S12, under nitrogen protection, lactic acid and catalyst are added to the reactor, the temperature is raised to 155°C for reaction for 2h, the temperature is further raised to 185°C for reaction for 2h, and the water separation quality is observed; the temperature is lowered to 140°C, the intermediate product 1I is added, stirred for 6h, cooled to room temperature, distilled under reduced pressure, and vacuum dried at 60°C for 6h to obtain the target product, i.e., plasticizer (average degree of polymerization is 5.4).
[0217] The intermediate product 1I and lactic acid are added at a molar ratio of epoxy group to carboxyl group of 1:5.
[0218] The amount of the catalyst used is 0.4% of the total mass of the reactants.
[0219] Its infrared data are as follows: 3382cm -1 :-OH exists and is significantly enhanced; 1735cm-1 :-C=O exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group does not exist; 1109cm -1 、801cm -1 :-Si-O- exists.
[0220] A method for preparing a vegetable oil-based resin comprises the following steps:
[0221] S21, tung oil, 3-mercaptopropionic acid, and photoinitiator 184 were added to dichloromethane A, and the mixture was irradiated with UV for 2 h at room temperature, and the mixture was washed with deionized water B for 3 times, and the organic phase was separated, and the organic phase was dried with anhydrous sodium sulfate A, filtered, and the filtrate was distilled under reduced pressure, and dried under vacuum at 40° C. for 12 h to obtain the intermediate product 2I;
[0222] The tung oil, 3-mercaptopropionic acid, dichloromethane A, deionized water B, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 5.0 mmol: 20 mL: 25 mL: 5 g;
[0223] The amount of the photoinitiator 184 used is 2.0% of the total mass of the reactants.
[0224] Its infrared data are as follows: 3377cm -1 :-OH exists; 1760cm -1 :-C=O exists; 2550cm -1 :-SH does not exist; 1621cm -1 :-C=C- does not exist.
[0225] S22, add the intermediate product 2I, glycidyl methacrylate, tetrabutylammonium bromide and hydroquinone to tetrahydrofuran, heat under reflux for 24 hours, cool to room temperature, add deionized water C, shake, add dichloromethane B for extraction, take the organic phase, dry it with anhydrous sodium sulfate, filter, take the filtrate, distill it under reduced pressure, and vacuum dry it at 40°C for 12 hours to obtain the target product, i.e., plant oil-based resin.
[0226] The intermediate product 2I, glycidyl methacrylate, tetrabutylammonium bromide, tetrahydrofuran, deionized water C, dichloromethane B, and anhydrous sodium sulfate are added in a ratio of 1 mmol: 1 mmol: 0.1 mmol: 5 mL: 10 mL: 20 mL: 1 g;
[0227] The amount of hydroquinone used is 0.1wt% of the mass of glycidyl methacrylate.
[0228] Its infrared data is as follows: 3376cm -1 :-OH exists; 1760cm-1 :-C=O (carboxyl) does not exist; 1735cm -1 :-C=O (ester group) exists; 1606cm -1 、811cm -1 :-C=C- exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group does not exist.
[0229] A method for preparing hyperbranched lactic acid acrylate comprises the following steps:
[0230] S31, adding plasticizer, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone into dichloromethane C, stirring at 80° C. for 6 h, distilling under reduced pressure, and vacuum drying at 40° C. for 12 h to obtain the target product, i.e., hyperbranched lactic acid acrylate.
[0231] The plasticizer and isocyanoethyl methacrylate are added at a molar ratio of hydroxyl group to isocyanoethyl methacrylate of 2.0:1;
[0232] The usage ratio of the plasticizer to dichloromethane C is 1 g:20 mL.
[0233] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0234] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0235] Its infrared data are as follows: 3382cm -1 :-OH exists and weakens; 1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0236] Example 3
[0237] The rest is the same as in Example 1, except that:
[0238] A method for preparing a plasticizer comprises the following steps:
[0239] S11, placing nano-silicon in ethyl acetate A, ultrasonically dispersing for 1 hour, adding epoxy silane coupling agent KH560 and deionized water A, slowly heating to 80°C, heating and stirring for 6 hours, after the reaction is completed, cooling to room temperature, filtering, washing with ethyl acetate B, and vacuum drying at 40°C to constant weight to obtain the target product, i.e., intermediate product 1I;
[0240] The dosage ratio of the nano silicon, ethyl acetate A, epoxy silane coupling agent, deionized water A, and ethyl acetate B is: 1.00 g: 50 mL: 5.0 g: 0.6 g: 200 mL.
[0241] Its infrared data is as follows: 3378cm -1 :-OH exists and weakens; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0242] S12, under nitrogen protection, lactic acid and catalyst are added into the reactor, the temperature is raised to 165°C for reaction for 2h, the temperature is further raised to 175°C for reaction for 4h, and the water separation quality is observed; the temperature is lowered to 120°C, the intermediate product 1I is added, stirred for 8h, cooled to room temperature, distilled under reduced pressure, and vacuum dried at 60°C for 6h to obtain the target product, i.e., plasticizer (average degree of polymerization is 9.7).
[0243] The intermediate product 1I and lactic acid are added at a molar ratio of epoxy group to carboxyl group of 1:10.
[0244] The amount of the catalyst used is 0.4% of the total mass of the reactants.
[0245] Its infrared data are as follows: 3382cm -1 :-OH exists and is significantly enhanced; 1735cm -1 :-C=O exists; 1265cm -1 、938cm -1 、801cm -1 : Epoxy group does not exist; 1109cm -1 、801cm -1 :-Si-O- exists.
[0246] A method for preparing a vegetable oil-based resin comprises the following steps:
[0247] S21, soybean oil, mercaptoethanol, and photoinitiator 184 were added to dichloromethane A, and the reaction was carried out under UV radiation at room temperature for 1 h, and the mixture was washed with deionized water B for 3 times, and the organic phase was separated, dried with anhydrous sodium sulfate A, filtered, and the filtrate was distilled under reduced pressure and dried in vacuum at 40°C for 12 h to obtain the intermediate product 2I;
[0248] The soybean oil, mercaptoethanol, dichloromethane A, deionized water B, and anhydrous sodium sulfate A are added in a ratio of 1 mmol: 3.0 mmol: 20 mL: 25 mL: 5 g;
[0249] The amount of the photoinitiator 184 used is 3.0% of the total mass of the reactants.
[0250] Its infrared data are as follows: 3381cm -1 :-OH exists; 2550cm -1 :-SH does not exist; 1621cm -1 :-C=C- does not exist.
[0251] S22, add the intermediate product 2I, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone to dichloromethane B, stir at 80°C for 6 hours, distill under reduced pressure, and vacuum dry at 40°C for 12 hours to obtain the target product, i.e., plant oil-based resin.
[0252] The intermediate product 2I and the acryloyl structure A are mixed in a molar ratio of 1:1 based on the reaction functional groups;
[0253] The ratio of the intermediate product 2I to dichloromethane B is 1 mmol:20 mL;
[0254] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0255] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0256] Its infrared data are as follows: 3381cm -1 :-OH does not exist; 2270cm -1 :-NCO does not exist; 1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists.
[0257] A method for preparing hyperbranched lactic acid acrylate comprises the following steps:
[0258] S31, adding a plasticizer, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone into dichloromethane C, stirring at 50° C. for 10 h, distilling under reduced pressure, and vacuum drying at 40° C. for 12 h to obtain the target product, i.e., hyperbranched lactic acid acrylate.
[0259] The plasticizer and isocyanoethyl methacrylate are added at a molar ratio of hydroxyl group to isocyanoethyl methacrylate of 10.0:1;
[0260] The usage ratio of the plasticizer to dichloromethane C is 1 g: 20 mL;
[0261] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0262] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0263] Its infrared data are as follows: 3382cm -1 :-OH exists and weakens; 1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists; 1109cm -1 、801cm -1 :-Si-O- exists.
[0264] Example 4
[0265] The rest is the same as in Example 1, except that:
[0266] A PLA-based tape comprises a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively;
[0267] The substrate comprises the following raw materials in parts by weight:
[0268] PLA 60 parts;
[0269] PBAT 40 parts;
[0270] 1.0 part of compatibilizer;
[0271] Plasticizer 5.0 parts;
[0272] 0.3 parts of antioxidant;
[0273] Lubricant 1.0 part;
[0274] The adhesive layer comprises the following raw materials in percentage by weight:
[0275] Hyperbranched lactic acid acrylate 35 parts;
[0276] 35 parts of vegetable oil-based resin;
[0277] 3.0 parts of functional monomer;
[0278] 3 parts of methacrylic acid;
[0279] 2 parts of 2-ethylhexyl acrylate;
[0280] 3 parts of glycidyl methacrylate;
[0281] 2 parts of hydroxyethyl methacrylate;
[0282] Photoinitiator TPO 2.0 parts;
[0283] 0.2 parts of defoaming agent;
[0284] 0.3 parts of leveling agent;
[0285] Solvent Residue.
[0286] A method for preparing a PLA-based adhesive tape comprises the following steps:
[0287] S51, preparation of substrate, i.e.
[0288] The raw materials are uniformly blended according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film (thickness of 50 μm);
[0289] The twin-screw extruder is set with the temperatures of zone 1 at 150°C, zone 2 at 160°C, zone 3 at 170°C, zone 4 at 185°C, die head temperature at 190°C, and casting temperature at 30°C.
[0290] The biaxial stretching parameters are: stretching ratio of 4.0; temperature of 90° C.; and speed of 60 mm / s.
[0291] The heat setting is performed at 90° C. for 20 minutes.
[0292] S52, coating a release layer, i.e.
[0293] Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling (the release layer thickness is 2 μm); and
[0294] S53, the other side of the substrate is coated with an adhesive layer, i.e.
[0295] The adhesive layer solution was prepared according to the ratio, and after adjusting the online viscosity, it was coated on the substrate by gravure, put into the drying tunnel, and the drying temperature was controlled at 80°C. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape (adhesive layer thickness of 14 μm) was obtained.
[0296] Example 5
[0297] The rest is the same as in Example 1, except that:
[0298] A PLA-based tape comprises a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively;
[0299] The substrate comprises the following raw materials in parts by weight:
[0300] PLA 80 parts;
[0301] PBAT 20 copies;
[0302] 0.5 parts of compatibilizer;
[0303] 10.0 parts of plasticizer;
[0304] 0.5 parts of antioxidant;
[0305] 0.5 parts of lubricant;
[0306] The adhesive layer comprises the following raw materials in percentage by weight:
[0307] Hyperbranched lactic acid acrylate 45 parts;
[0308] 25 parts of vegetable oil-based resin;
[0309] 2.0 parts of functional monomer;
[0310] 1 part of methacrylic acid;
[0311] 2 parts of 2-ethylhexyl acrylate;
[0312] 1 part of glycidyl methacrylate;
[0313] 1 part of hydroxyethyl methacrylate;
[0314] Photoinitiator 1173 4.0 parts;
[0315] Defoaming agent 0.1 part;
[0316] 0.1 part of leveling agent;
[0317] Solvent Residue.
[0318] A method for preparing a PLA-based adhesive tape comprises the following steps:
[0319] S51, preparation of substrate, i.e.
[0320] The raw materials are uniformly blended according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film (thickness of 50 μm);
[0321] The twin-screw extruder has set temperatures of 165°C in zone 1, 175°C in zone 2, 185°C in zone 3, 190°C in zone 4, 200°C in die head temperature, and 50°C in casting temperature.
[0322] The biaxial stretching parameters are: stretching ratio of 3.0; temperature of 70°C; speed of 100 mm / s;
[0323] The heat setting is performed at 100° C. for 10 minutes.
[0324] S52, coating a release layer, i.e.
[0325] Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling (the release layer thickness is 2 μm); and
[0326] S53, the other side of the substrate is coated with an adhesive layer, i.e.
[0327] The adhesive layer solution was prepared according to the ratio, and after adjusting the online viscosity, it was coated on the substrate by gravure, put into the drying tunnel, and the drying temperature was controlled at 45°C. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape (adhesive layer thickness of 14 μm) was obtained.
[0328] The following comparative examples are compared with specific embodiment 1:
[0329] Comparative Example 1
[0330] The rest is the same as in Example 1, except that:
[0331] No plasticizer is added to the raw material formula of the PLA-based adhesive tape substrate.
[0332] Comparative Example 2
[0333] The rest is the same as in Example 1, except that:
[0334] A method for preparing a plasticizer comprises the following steps:
[0335] S31, under nitrogen protection, lactic acid and catalyst were added into the reactor, the temperature was raised to 160°C for reaction for 2h, the temperature was further raised to 180°C for reaction for 2.5h, and the water quality was observed; the temperature was lowered to room temperature, vacuum distilled, and vacuum dried at 60°C for 6h to obtain the target product, i.e., plasticizer (average degree of polymerization was 7.9).
[0336] The amount of the catalyst used is 0.4% of the total mass of the reactants.
[0337] Its infrared data are as follows: 3382cm -1 :-OH exists; 1760cm -1 、1735cm -1 :-C=O exists.
[0338] Comparative Example 3
[0339] The rest is the same as in Example 1, except that:
[0340] The PLA-based tape adhesive layer raw material formula does not contain hyperbranched lactic acid acrylate; and the total number of hyperbranched lactic acid acrylate and plant oil-based resin is 70 parts.
[0341] Comparative Example 4
[0342] The rest is the same as in Example 1, except that:
[0343] A method for preparing lactic acid acrylate comprises the following steps:
[0344] S31, under nitrogen protection, add lactic acid and catalyst into the reactor, heat to 160°C for reaction for 2h, continue to heat to 180°C for reaction for 2.5h, observe the quality of water separation; cool to room temperature, distill under reduced pressure, and vacuum dry at 60°C for 6h to obtain lactic acid oligomers (average degree of polymerization: 7.9).
[0345] The amount of the catalyst used is 0.4% of the total mass of the reactants.
[0346] Its infrared data are as follows: 3382cm -1 :-OH exists; 1760cm -1 、1735cm -1 :-C=O exists.
[0347] S32, add lactic acid oligomer, isocyanoethyl methacrylate, dibutyltin dilaurate and hydroquinone into dichloromethane C, stir at 60°C for 8h, distill under reduced pressure, and vacuum dry at 40°C for 12h to obtain lactic acid monoacrylate.
[0348] The lactic acid oligomer and isocyanoethyl methacrylate are added in a molar ratio of hydroxyl group to isocyanoethyl methacrylate of 1:1;
[0349] The usage ratio of the plasticizer to dichloromethane C is 1 g:20 mL.
[0350] The amount of dibutyltin dilaurate is 0.5wt% of isocyanatoethyl methacrylate;
[0351] The amount of hydroquinone used is 0.1wt% of isocyanoethyl methacrylate.
[0352] Its infrared data are as follows: 3381cm -1 :-OH exists and weakens; 1760cm -1 、1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists.
[0353] S33, lactic acid monoacrylate, glycidyl methacrylate, triphenylphosphine, and hydroquinone are added to N,N-dimethylformamide, stirred at 100° C. for 15 h, distilled under reduced pressure, and vacuum dried at 40° C. for 12 h to obtain lactic acid diacrylate.
[0354] The dosage ratio of lactic acid monoacrylate, glycidyl methacrylate, and N,N-dimethylformamide is 1 mmol: 1 mmol: 20 mL;
[0355] The amount of triphenylphosphine used is 0.4% of the total mass of the reactants;
[0356] The amount of hydroquinone used is 0.1% of the total mass of the reactants.
[0357] Its infrared data are as follows: 3380cm -1 :-OH exists; 1735cm -1 、1680cm -1 :-C=O exists; 1606cm -1 、811cm -1 :-C=C- exists and is enhanced.
[0358] Comparative Example 5
[0359] The rest is the same as in Example 1, except that:
[0360] The raw material formula of the PLA-based tape adhesive layer does not contain any plant oil-based resin; and the total number of parts of the hyperbranched lactic acid acrylate and the plant oil-based resin is 70 parts.
[0361] Comparative Example 6
[0362] The rest is the same as in Example 1, except that:
[0363] The vegetable oil-based resin was replaced with soybean oil.
[0364] Comparative Example 7
[0365] The rest is the same as in Example 1, except that:
[0366] No functional monomer is added to the raw material formula of the adhesive layer of the PLA-based tape.
[0367] Comparative Example 8
[0368] The rest is the same as in Example 1, except that:
[0369] The preparation method of the PLA-based adhesive tape is not subjected to a biaxial stretching process.
[0370] The physical properties of the PLA-based tapes in the embodiments of the present invention and the comparative examples are shown in Table 1.
[0371] Table 1 Physical test performance of each embodiment
[0372]
[0373]
[0374] First, it can be concluded from Examples 1-5 in Table 1 that the PLA-based adhesive tape of the present invention has excellent mechanical properties and high adhesive properties.
[0375] Second, it can be observed from Example 1 and Comparative Examples 1-2 that the PLA-based tape of the present invention uses a homemade plasticizer in the substrate, which has a positive effect on improving the mechanical properties of the PLA substrate;
[0376] It can be observed from Example 1 and Comparative Examples 3-4 that in the PLA-based tape of the present invention, the self-made hyperbranched lactic acid acrylate is used in the adhesive layer, which has excellent compatibility with the substrate, as reflected in the absence of residual adhesive; and has excellent bonding strength to the adherend;
[0377] It can be observed from Example 1 and Comparative Examples 5-6 that the vegetable oil-based ones can improve the bonding strength to a certain extent;
[0378] It can be observed from Example 1 and Comparative Example 7 that the functional monomer containing a catechol structure has a positive effect on improving the bonding strength, especially in an environment with high humidity.
[0379] It can be observed from Example 1 and Comparative Example 8 that the PLA-based tape of the present invention has more excellent mechanical properties after biaxial stretching.
[0380] In summary, the PLA-based adhesive tape provided by the present invention, on the one hand, through molecular design, a plasticizer applied to the substrate and a main resin and functional monomer applied to the adhesive layer are prepared by self-production; on the other hand, through formula design, after the substrate is prepared by extrusion and biaxial stretching process, the adhesive tape is prepared by double-sided coating. The PLA-based adhesive tape has excellent mechanical properties and adhesive properties.
[0381] The test method is as follows:
[0382] (1) Mechanical properties: Tested according to the method described in GB / T 1040.3-2006.
[0383] (2) 180° peel strength: tested according to the method described in GB / T 2792-2014.
[0384] (3) Adhesion: According to GB / T 4851-2014, the test was conducted using method B, with the relative humidity being 80%.
[0385] (4) Check whether there is residual glue after peeling off: visual inspection. The marking method for whether there is residual glue is: no residual glue, marked as "○"; small area of residual glue, marked as "◎"; large area of residual glue, marked as "●".
[0386] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing a plasticizer, characterized in that: The following steps are involved: S11, performing silylation coupling reaction on nano-silicon and epoxy silane coupling agent to obtain intermediate product 1I; S12, subjecting the intermediate product 1I to esterification and ring-opening reaction with lactic acid to obtain the target product, i.e., the plasticizer.
2. The method for preparing a compatibilizer according to claim 1, characterized in that: The usage ratio of the nano silicon to the epoxy silane coupling agent is 1g:5.0-7.0g.
3. The method for preparing a compatibilizer according to claim 1, characterized in that: The intermediate product II and lactic acid are added in a molar ratio of epoxy group to carboxyl group of 1:5-10.
4. A plasticizer, characterized in that Prepared by the preparation method of the plasticizer according to any one of claims 1 to 3.
5. A method for preparing a plant oil-based resin, characterized in that: The following steps are involved: S21, click reaction of vegetable oil with thiol derivatives to obtain intermediate 2I; S22, coupling reaction of the intermediate product 2I with the acryloyl structure A to obtain the target product, i.e., the plant oil-based resin.
6. The method for preparing the plant oil-based resin according to claim 5, characterized in that: The vegetable oil and the thiol derivative are added in a molar ratio of 1:3-5; and The vegetable oil is a drying oil or a semi-drying oil.
7. The method for preparing the plant oil-based resin according to claim 5, characterized in that: The intermediate product 2I and the acryloyl structure A are mixed in a molar ratio of 1:1 based on the reaction functional groups; and The acryl structure A contains a functional group that can react with the hydroxyl structure.
8. A plant oil-based resin, characterized in that: Prepared by the preparation method of the plant oil-based resin as claimed in any one of claims 5 to 7.
9. A method for preparing hyperbranched lactic acid acrylate, characterized in that: The following steps are involved: S31, coupling reaction of the plasticizer with the acryloyl structure B to obtain the target product, namely, hyperbranched lactic acid acrylate.
10. The method for preparing the functional monomer according to claim 9, characterized in that: The plasticizer and the acryl structure B are added at a molar ratio of hydroxyl group to acryl structure B of 2.0-10.0:1; and The acryl structure B contains a functional group that can react with the hydroxyl structure.
11. A hyperbranched lactic acid acrylate, characterized in that: The invention is prepared by the method for preparing hyperbranched lactic acid acrylate according to claim 9 or 10.
12. A method for preparing a functional monomer, characterized in that: The following steps are involved: S41, subjecting catechin to a ring-opening reaction with glycidyl methacrylate to obtain a target product, namely a functional monomer.
13. The method for preparing the functional monomer according to claim 12, characterized in that: The catechin and glycidyl methacrylate are added in a molar ratio of 1:
1.
14. A functional monomer, characterized in that: Prepared by the method for preparing the functional monomer as claimed in claim 12 or 13.
15. A PLA-based adhesive tape, characterized in that: It comprises a substrate, a release layer and an adhesive layer; the release layer and the adhesive layer are coated on both sides of the substrate respectively; The substrate comprises the following raw materials in parts by weight: PLA 60-80 parts; PBAT 20-40 parts; Compatibilizer 0.5-1.0 part; Plasticizer 5.0-10.0 parts; Antioxidant 0.3-0.5 parts; Lubricant 0.5-1.0 part; Among them, the total mass of PLA and PBAT is 100 parts; The adhesive layer comprises the following raw materials in percentage by weight: Hyperbranched lactic acid acrylate 35-45 parts; 25-35 parts of vegetable oil-based resin; 2.0-3.0 parts of functional monomer; 5-10 parts of diluent; Photoinitiator 2.0-4.0 parts; Defoaming agent 0.1-0.2 parts; Leveling agent 0.1-0.3 parts; Solvent Residue.
16. A method for preparing a PLA-based adhesive tape, characterized in that: The steps include: S51, preparation of substrate, i.e. The raw materials are mixed evenly according to the ratio, added to the extruder, heated and melted, extruded through a die head, and the melt is attached to the surface of a casting roll for cooling to obtain a cast sheet; biaxial stretching is performed, and then heat setting is performed to obtain a biaxially oriented film; S52, coating a release layer, i.e. Using a two-roll transfer coating method, coating silicone on one side of the base film layer, drying by far-infrared radiation drying, and winding after drying and cooling; and S53, the other side of the substrate is coated with an adhesive layer, i.e. The adhesive layer solution is prepared according to the ratio, and after adjusting the online viscosity, it is coated on the substrate by gravure, put into the drying tunnel, and the drying temperature is controlled at 45-80℃. After UV curing, cooling, winding, and slitting, the required width of PLA-based tape is obtained.