Clay-based catalyst as well as preparation method and application thereof

By adjusting the ratio of acidic sites and alkaline sites in clay-based catalysts and combining metal oxide modification, the problems of catalyst channel blockage and activity reduction are solved, and the conversion rate of tetrahydrofuran and the long-term effectiveness of the catalyst are improved.

CN118930837APending Publication Date: 2024-11-12SHANGHAI HUAFON NEW MATERIAL R&D TECH CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411253936.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing catalysts have problems of catalyst pore blockage during the ring-opening polymerization of tetrahydrofuran, resulting in a decrease in catalytic activity and an increase in cost, and it is difficult to effectively solve the problem of blockage caused by macromolecules.

Method used

By adjusting the content ratio of acidic sites and alkaline sites in clay-based catalysts, the acidic sites content is increased to inhibit the formation of macromolecular chains, and combining metal oxide modifications to control site distribution, ensuring catalyst activity and conversion.

Benefits of technology

It effectively reduces the blockage of the catalyst channel, improves the catalytic activity and the conversion rate of tetrahydrofuran, reduces the cost of catalyst replacement, and realizes the long-term use of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005033372650000191
    Figure BDA0005033372650000191
  • Figure BDA0005033372650000211
    Figure BDA0005033372650000211
  • Figure BDA0005033372650000221
    Figure BDA0005033372650000221
Patent Text Reader

Abstract

The invention relates to a clay-based catalyst as well as a preparation method and application thereof. The content of alkaline sites in the clay-based catalyst is 0.8 mmol / g to 1.8 mmol / g; the content of acidic sites in the clay-based catalyst is less than or equal to 1.8 mmol / g; the content of the acidic sites is more than 0.9 time of the content of the alkaline sites. According to the clay-based catalyst provided by the invention, the content of alkaline sites in the clay-based catalyst is controlled, and the content ratio of the acidic sites to the alkaline sites is increased at the same time, so that the catalytic activity gain caused by the increase of the overall acidic site content exceeds the benefit reduction effect caused by the increase of the alkaline sites, and the inhibition effect of the increase of the alkaline sites on macromolecular chains is retained; the catalyst pore channel blockage caused by macromolecule generation can be reduced while the conversion rate is ensured, so that the catalytic activity is ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, in particular to a catalyst for catalyzing ring-opening polymerization, and in particular to a clay-based catalyst and a preparation method and application thereof. Background Art

[0002] Polytetrahydrofuran (PTMEG) is an important raw material for the production of spandex, polyurethane elastomers and ester-ether copolymers, and is widely used in industrial production fields such as petrochemicals, textiles, and machinery. PTMEG is generally produced by the ring-opening polymerization of tetrahydrofuran monomers. Commonly used catalysts include strong proton acids based on homogeneous reactions. However, this type of process has problems such as equipment corrosion, catalyst recovery, and environmental pollution caused by acidic and salty wastewater.

[0003] The use of heterogeneous solid acid catalysts not only has the advantages of being environmentally friendly and having mild reaction conditions, but also can overcome the above-mentioned equipment corrosion and catalyst separation problems. Clay-based catalysts are a type of solid acid catalyst that can be used for cracking reactions, alkylation reactions, esterification reactions, and hydration reactions. Common clay-based catalysts use clays such as attapulgite, montmorillonite, kaolin, or halloysite.

[0004] US4127513A discloses a method for the ring-opening polymerization of tetrahydrofuran, wherein the catalyst used is acidified montmorillonite treated with sulfuric acid, and the use of the catalyst improves the polymerization yield.

[0005] CN1684762A discloses a solid acid catalyst having a BET specific surface area of ​​at least 160 m 2 / g, and the pore volume of N2 with pore diameter in the range of 2-200nm is at least 0.2m 3 / g, and at least 0.1cm in the N2 pore volume 3 / g is composed of pores with a pore diameter in the range of 5-50nm.

[0006] Acid-activated clay-based catalysts have high specific surface area and adjustable surface acid centers, and are non-corrosive and non-toxic. They are easy to separate and environmentally friendly during the production process, and show good development potential in catalytic tetrahydrofuran polymerization and other reactions. However, the reaction of tetrahydrofuran polymerization to produce polytetrahydrofuran occurs on the surface and pores of the catalyst, and the polymerization process is a process of converting small molecules into polymers. The existing technology generally has the problem of long polymer chains blocking the catalyst pores.

[0007] The catalytic activity of the catalyst will decrease after the pores are blocked, but if the catalyst is frequently replaced, the cost will rise rapidly. By changing the pore structure and increasing the pore size, the degree of pore blockage can be reduced to a certain extent, the activity of the catalyst can be increased, and the conversion rate of PTMEG can be increased from 40% to 44%, but the activity of the catalyst still has room for improvement. For example, if the formation of macromolecular products in the pores can be avoided, the problem of catalyst blockage can be solved from the source, thereby improving the catalyst activity.

[0008] Therefore, it is necessary to provide a clay-based catalyst with high activity for catalyzing ring-opening polymerization, especially tetrahydrofuran ring-opening polymerization, and a preparation method and application thereof. Summary of the invention

[0009] The object of the present invention is to provide a clay-based catalyst and a preparation method and application thereof, wherein the clay-based catalyst can inhibit the synthesis of macromolecular chains, reduce the clogging of catalyst channels caused by the production of macromolecules while ensuring the conversion rate, and ensure the catalytic activity of the catalyst.

[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:

[0011] In a first aspect, the present invention provides a clay-based catalyst, wherein the basic site content in the clay-based catalyst is 0.8 mmol / g to 1.8 mmol / g;

[0012] The acidic site content in the clay-based catalyst is ≤1.8 mmol / g;

[0013] The acidic site content is 0.9 times or more of the basic site content.

[0014] The inventors found that the content of acidic sites is the cause of the blockage of long-chain polymers in the pores, which is specifically manifested in a certain amount of weight loss in the clay-based catalyst during the TGA test at 200°C to 400°C. This temperature is not the decomposition temperature of the clay-based catalyst, so the weight loss comes from the polymer residue in the pores. When the acidic site content and the basic site content in the clay-based catalyst are adjusted, the residue of the long-chain polymer obtained by the TGA test changes.

[0015] During the polymerization reaction, the alkaline site does not catalyze the chain growth reaction, but the alkaline site is easy to combine with water, resulting in an increase in the water content near the clay-based catalyst. The prior art usually reduces the content of the alkaline site to reduce the adverse effect of the alkaline site on the catalytic activity. The present invention utilizes the characteristic that the inhibitory effect of the alkaline site on the growth of the polymer chain is greater than the inhibitory effect on the growth of the low molecular weight chain, increases the content of the alkaline site in the clay-based catalyst, and simultaneously increases the content ratio of the acidic site to the alkaline site, so that the catalytic activity gain brought by the overall increase in the acidic site content exceeds the loss effect brought by the increase in the alkaline site, and retains the inhibitory effect of the increase in the alkaline site on the macromolecular chain, which can reduce the catalyst pore blockage caused by the production of macromolecules while ensuring the conversion rate, thereby ensuring the catalytic activity.

[0016] Preferably, the acidic sites include strong acidic sites and weak acidic sites;

[0017] The ratio of the content of the weak acid sites to the content of the strong acid sites is 0.7-2.

[0018] The present invention divides the acid sites into strong acid sites and weak acid sites according to the different peak positions of the acid sites in the TPD test spectrum, that is, the acid sites with peak intensity at 400°C and below are weak acid sites, and the acid sites with peak intensity exceeding 400°C are strong acid sites.

[0019] Preferably, the clay-based catalyst comprises a clay matrix, a first metal oxide and a second metal oxide;

[0020] The first metal oxide is an oxide capable of increasing the acid site content of the clay-based catalyst;

[0021] The second metal oxide is an oxide capable of increasing the basic site content of the clay-based catalyst.

[0022] Preferably, the first metal oxide includes any one of iron oxide, zirconium oxide, titanium dioxide, cobalt oxide, nickel oxide, copper oxide, zinc oxide or molybdenum oxide, or a combination of at least two thereof.

[0023] Preferably, the second metal oxide comprises any one of lanthanum oxide, cerium oxide, samarium oxide or yttrium oxide, or a combination of at least two thereof;

[0024] Preferably, the clay matrix includes any one of attapulgite, montmorillonite, kaolin or halloysite, or a combination of at least two of them.

[0025] Preferably, the clay matrix is ​​acidified clay.

[0026] Preferably, the surface area of ​​the acidified clay is ≥150m 2 / g, pore diameter ≥3nm, pore volume ≥0.25mL / g.

[0027] In a second aspect, the present invention provides a method for preparing the clay-based catalyst as described in the first aspect, the preparation method comprising the following steps:

[0028] Mixing a clay matrix, a binder and a mixed metal salt solution according to a formula, and then kneading the obtained slurry into a blank; calcining the obtained blank to obtain the clay-based catalyst;

[0029] The mixed metal salt solution is a solution comprising a first metal salt and a second metal salt;

[0030] The first metal salt and the second metal salt are converted into the first metal oxide and the second metal oxide after calcination.

[0031] Preferably, the calcination temperature is 300° C. to 600° C., and the calcination time is 2 h to 10 h.

[0032] Preferably, the binder includes any one of boehmite, pseudo-boehmite, silica sol or alumina sol, or a combination of at least two of them.

[0033] In a third aspect, the present invention provides a use of the clay-based catalyst as described in the first aspect, wherein the clay-based catalyst is used to catalyze the synthesis of polytetrahydrofuran.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] During the polymerization reaction, the alkaline sites do not catalyze the chain growth reaction, but the alkaline sites are easily combined with water, resulting in an increase in the water content near the clay-based catalyst. The prior art usually reduces the alkaline site content to reduce the adverse effects of the alkaline sites on the catalytic activity. The present invention utilizes the characteristic that the inhibitory effect of the alkaline sites on the growth of high molecular chains is greater than the inhibitory effect on the growth of low molecular chains, increases the content of alkaline sites in the clay-based catalyst, and simultaneously increases the content ratio of the acidic sites to the alkaline sites, so that the catalytic activity gain brought by the overall increase in the acidic site content exceeds the loss effect brought by the increase in the alkaline sites, and retains the inhibitory effect of the increase in the alkaline sites on the macromolecular chains, which can reduce the catalyst pore blockage caused by the production of macromolecules while ensuring the conversion rate, thereby ensuring the catalytic activity. DETAILED DESCRIPTION

[0036] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0037] A certain embodiment of the present invention provides a clay-based catalyst, wherein the basic site content in the clay-based catalyst is 0.8 mmol / g to 1.8 mmol / g;

[0038] The acidic site content in the clay-based catalyst is ≤1.8 mmol / g;

[0039] The acidic site content is 0.9 times or more of the basic site content.

[0040] The inventors found that the content of acidic sites is the cause of the blockage of long-chain polymers in the pores, which is specifically manifested in a certain amount of weight loss in the clay-based catalyst during the TGA test at 200°C to 400°C. This temperature is not the decomposition temperature of the clay-based catalyst, so the weight loss comes from the polymer residue in the pores. When the acidic site content and the basic site content in the clay-based catalyst are adjusted, the residue of the long-chain polymer obtained by the TGA test changes.

[0041] During the polymerization reaction, the alkaline site does not catalyze the chain growth reaction, but the alkaline site is easy to combine with water, resulting in an increase in the water content near the clay-based catalyst. The prior art usually reduces the content of the alkaline site to reduce the adverse effect of the alkaline site on the catalytic activity. The present invention utilizes the characteristic that the inhibitory effect of the alkaline site on the growth of the polymer chain is greater than the inhibitory effect on the growth of the low molecular weight chain, increases the content of the alkaline site in the clay-based catalyst, and simultaneously increases the content ratio of the acidic site to the alkaline site, so that the catalytic activity gain brought by the overall increase in the acidic site content exceeds the loss effect brought by the increase in the alkaline site, and retains the inhibitory effect of the increase in the alkaline site on the macromolecular chain, which can reduce the catalyst pore blockage caused by the production of macromolecules while ensuring the conversion rate, thereby ensuring the catalytic activity.

[0042] The basic site content in the clay-based catalyst is 0.8 mmol / g to 1.8 mmol / g, for example, 0.8 mmol / g, 0.9 mmol / g, 1 mmol / g, 1.2 mmol / g, 1.5 mmol / g, 1.6 mmol / g or 1.8 mmol / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0043] In the present invention, the content of basic sites in the clay-based catalyst needs to be above 0.8 mmol / g, otherwise it will have little effect on reducing the excessively long molecular chains; but at the same time, the content of basic sites needs to be below 1.8 mmol / g, otherwise it will affect the catalytic efficiency of the clay-based catalyst.

[0044] The acid site content in the clay-based catalyst is ≤1.8mmol / g, for example, it can be 0.75mmol / g, 0.8mmol / g, 0.9mmol / g, 1mmol / g, 1.2mmol / g, 1.4mmol / g, 1.5mmol / g, 1.6mmol / g or 1.8mmol / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0045] The acidic site content is more than 0.9 times the basic site content, for example, it can be 0.9 times, 1 times, 1.2 times, 1.4 times, 1.5 times, 1.6 times or 1.8 times, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] In the present invention, if the ratio of the acidic site content to the basic site content is less than 0.9, the adverse effect of the introduction of basic sites on the catalytic effect cannot be offset.

[0047] In certain preferred embodiments, the acidic sites include strong acidic sites and weak acidic sites;

[0048] The ratio of the content of the weak acid sites to the content of the strong acid sites is 0.7-2, for example, 0.7, 0.72, 0.8, 1, 1.2, 1.5, 1.8 or 2, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0049] The present invention divides the acid sites into strong acid sites and weak acid sites according to the different peak positions of the acid sites in the TPD test spectrum, that is, the acid sites with peak intensity at 400°C and below are weak acid sites, and the acid sites with peak intensity exceeding 400°C are strong acid sites.

[0050] The acid sites in clay-based catalysts are all conducive to the reaction. However, when the proportion of weak acid sites in the acid sites is reduced, it is easy to induce the formation of high molecular weight products and cause blockage. Moreover, strong acid sites cannot be completely removed, otherwise it will cause serious structural collapse and deactivate the catalyst. For the above reasons, when modifying the acid active center, it is necessary to control the ratio of weak acid sites to strong acid sites to 0.7-2.

[0051] The clay-based catalyst comprises a clay matrix, a first metal oxide and a second metal oxide;

[0052] The first metal oxide is an oxide capable of increasing the acid site content of the clay-based catalyst;

[0053] The second metal oxide is an oxide capable of increasing the basic site content of the clay-based catalyst.

[0054] The first metal oxide in the clay-based catalyst of the present invention is an oxide that increases the acidic site content of the clay-based catalyst, which can enhance the catalytic activity of the clay-based catalyst, but it also easily leads to the production of polymers with excessively long molecular chains, and therefore, needs to be used in conjunction with the second metal oxide.

[0055] The second metal oxide in the clay-based catalyst of the present invention is an oxide that increases the basic site content of the clay-based catalyst, which can increase the weakly acidic sites and basic sites in the clay-based catalyst. When used in combination with the first metal oxide, the basic site content in the clay-based catalyst can be controlled to be 0.8 mmol / g to 1.5 mmol / g, the acidic site content is ≤1.5 mmol / g, and the acidic site content is more than 0.9 times the basic site content.

[0056] In certain embodiments, the first metal oxide comprises any one of iron oxide, zirconium oxide, titanium dioxide, cobalt oxide, nickel oxide, copper oxide, zinc oxide or molybdenum oxide, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of iron oxide and zirconium oxide, a combination of titanium dioxide and cobalt oxide, a combination of nickel oxide and copper oxide, a combination of copper oxide and zinc oxide, a combination of iron oxide, titanium dioxide and nickel oxide, a combination of cobalt oxide, copper oxide and zinc oxide, or a combination of iron oxide, zirconium oxide, titanium dioxide, cobalt oxide, nickel oxide, copper oxide and zinc oxide.

[0057] In certain embodiments, the second metal oxide comprises any one of lanthanum oxide, cerium oxide, samarium oxide or yttrium oxide, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of lanthanum oxide and cerium oxide, a combination of cerium oxide and samarium oxide, a combination of samarium oxide and yttrium oxide, a combination of lanthanum oxide, cerium oxide and samarium oxide, a combination of cerium oxide, samarium oxide and yttrium oxide, or a combination of lanthanum oxide, cerium oxide, samarium oxide and yttrium oxide.

[0058] In certain embodiments, the first metal oxide accounts for less than 8 wt % of the clay-based catalyst.

[0059] In certain embodiments, the second metal oxide is less than 5 wt % of the clay-based catalyst.

[0060] In certain embodiments, the total mass of the first metal oxide and the second metal oxide is less than 13 wt % of the clay-based catalyst.

[0061] In certain embodiments, the clay matrix includes any one of attapulgite, montmorillonite, kaolin or halloysite, or a combination of at least two of them. Typical but non-limiting combinations include a combination of attapulgite and montmorillonite, a combination of halloysite and kaolin, a combination of montmorillonite and halloysite, or a combination of attapulgite, montmorillonite, kaolin and halloysite.

[0062] In certain embodiments, the clay matrix is ​​acidified clay.

[0063] The initial conversion rate of the unmodified acidified clay itself will seriously affect the conversion rate of the modified clay-based catalyst. Even after the modification, the clay matrix with too low initial conversion rate cannot obtain a high conversion rate. On the other hand, the specific surface area, pore size and pore volume of the acidified clay determine the specific surface area, pore size and pore volume of the modified clay-based catalyst. The present invention does not specifically limit the source of the acidified clay. For example, the acidified clay comes from the purchase or acidification of the clay, so that the specific surface area, pore size, pore volume and initial conversion rate of the clay after acidification modification meet the requirements. If the unacidified clay itself has an initial conversion rate that meets the requirements, and after the acid-base active center is modified, its specific surface area, pore size and pore volume meet the control requirements, then this type of clay can also be used as a catalyst clay matrix. Although this type of clay has not been substantially acidified, it also belongs to the concept of the acidified clay of the present invention.

[0064] In certain embodiments, the surface area of ​​the acidified clay is ≥ 150 m 2 / g, pore diameter ≥3nm, pore volume ≥0.25mL / g.

[0065] The specific surface area of ​​the acidified clay is ≥150m 2 / g, for example, it can be 150m 2 / g, 160m 2 / g, 180m 2 / g, 190m 2 / g, 200m 2 / g or 210m 2 / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0066] The pore size of the acidified clay is ≥ 3 nm, for example, it can be 3 nm, 4 nm, 5 nm, 6 nm or 8 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0067] The pore volume of the acidified clay is ≥ 0.25 mL / g, for example, it can be 0.25 mL / g, 0.27 mL / g, 0.28 mL / g, 0.3 mL / g or 0.35 mL / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0068] The specific surface area of ​​the acidified clay affects the activity of the clay-based catalyst. If the specific surface area of ​​the acidified clay is too small, the conversion rate of tetrahydrofuran will be too low. The larger the pore size and pore volume of the acidified clay, the more conducive it is for the synthesized macromolecular polytetrahydrofuran to separate from the pores, so as to reduce the risk of pore blockage. The larger the specific surface area of ​​the acidified clay, the smaller the pore size and pore volume of the acidified clay, and the two restrict each other. In the present invention, the surface area of ​​the acidified clay is ≥150m 2 / g, pore diameter ≥3nm, and pore volume ≥0.25mL / g can obtain the best tetrahydrofuran conversion rate and clay-based catalyst life.

[0069] The specific surface area, pore diameter and pore volume refer to the specific surface area, pore diameter and pore volume of the acidified clay after being modified by the first metal oxide and the second metal oxide.

[0070] The testing methods for the specific surface area, pore volume and pore diameter include but are not limited to:

[0071] The nitrogen isothermal adsorption-desorption curve data of the test material can be obtained by a conventional fully automatic specific surface and porosity analyzer. The specific surface area, pore volume and pore size data of the corresponding sample can be obtained by analyzing the curve information. A typical operation process is to place 100 mg of sample in a sample tube, evacuate and heat to 200 ° C, desorb for 12 hours to remove the gas adsorbed on the surface, and then backfill with nitrogen protection and cool to room temperature. After the second weighing to record the weight before and after desorption, the sample tube is transferred to the analysis station and suspended. Liquid nitrogen is filled into a container with strong heat preservation effect such as a Dewar flask, and the sample tube is placed vertically in a liquid nitrogen environment and installed with a heat preservation cover. The nitrogen adsorption amount of the sample is measured by the software at a preset pressure point to obtain the adsorption isotherm. The ordinate of this curve is the mass (or volume) of nitrogen adsorbed by a unit mass of the sample under constant temperature conditions (liquid nitrogen temperature); its abscissa is the relative pressure P / P0, where P is the actual pressure of the gas and P0 is the saturated vapor pressure of the gas at this temperature. By processing data with a computer, the specific surface area, pore volume and average pore diameter can be calculated from the adsorption isotherm based on the corresponding mathematical model.

[0072] In certain embodiments, the initial conversion rate of the acidified clay is ≥ 25%.

[0073] The initial conversion rate of the acidified clay is ≥25%, for example, it can be 25%, 28%, 30%, 35%, 38%, 40% or 44%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0074] The initial conversion rate refers to the conversion rate of catalyzing polytetrahydrofuran when the clay or acidified clay is not modified by the first metal oxide and the second metal oxide. The test method of the conversion rate includes but is not limited to:

[0075] 1.6g of the acidified clay sample to be tested is added to a raw material containing 1.6g of acetic anhydride and 40g of tetrahydrofuran, and reacted at 40°C for 6h; the purity of the tetrahydrofuran is ≥99.9wt%, and the water content is less than 200ppm; after the reaction is completed, the polymer is separated by rotary evaporation, and the rotary evaporation conditions are 150°C oil bath environment, 10mbar pressure rotary evaporation for 30min, and then the conversion rate is calculated. The mass m0 (in g) of the polymer separated by rotary evaporation is measured, and the conversion rate Y0 = (m0 / 41.6) × 100%.

[0076] The method is also applicable to the conversion rate of the synthesis process when the clay-based catalyst modified by metal oxide is used to catalyze polytetrahydrofuran. When determining the conversion rate of the clay-based catalyst modified by metal oxide, the conversion rates Y1 and Y2 after the first use and the tenth use of the catalyst are respectively determined, wherein the mass m1 (in g) of the polymer separated after the first polymerization, then the conversion rate Y1=(m1 / 41.6)×100%; the tenth use is to collect the separated clay-based catalyst after the reaction is completed, and put it into the raw material containing 1.6g acetic anhydride and 40g tetrahydrofuran again, and repeat it ten times under the same reaction conditions, and perform TGA analysis on the catalyst collected for the tenth use, and determine the level of macromolecular residues in the catalyst and the mass m2 (in g) of the polymer separated by rotary evaporation after the tenth catalyst use reaction, then the conversion rate Y2 of the tenth catalyst use=(m2 / 41.6)×100%.

[0077] A certain embodiment of the present invention provides a method for preparing the clay-based catalyst described in certain embodiments, and the preparation method comprises the following steps:

[0078] Mixing a clay matrix, a binder and a mixed metal salt solution according to a formula, and then kneading the obtained slurry into a blank; calcining the obtained blank to obtain the clay-based catalyst;

[0079] The mixed metal salt solution is a solution comprising a first metal salt and a second metal salt;

[0080] The first metal salt and the second metal salt are converted into the first metal oxide and the second metal oxide after calcination.

[0081] The mixed metal salt solution is obtained by dissolving a first metal oxide and / or a first metal oxide precursor, and a second metal oxide and / or a second metal oxide precursor into an acidic solvent; the acidic solvent includes an organic acid and / or an inorganic acid.

[0082] Exemplarily, the organic acid includes any one of citric acid, acetic acid or formic acid, or a combination of at least two of them. Typical but non-limiting combinations include a combination of citric acid and acetic acid, a combination of acetic acid and formic acid, a combination of citric acid and formic acid, or a combination of citric acid, acetic acid and formic acid.

[0083] Exemplarily, the inorganic acid includes any one of nitric acid, hydrochloric acid or sulfuric acid, or a combination of at least two thereof. Typical but non-limiting combinations include a combination of nitric acid and hydrochloric acid, a combination of hydrochloric acid and sulfuric acid, a combination of nitric acid and sulfuric acid, or a combination of nitric acid, hydrochloric acid and sulfuric acid.

[0084] Exemplarily, the first metal oxide precursor is a metal salt corresponding to the same metal; for example, when the first metal oxide is iron oxide, the corresponding first metal oxide precursor includes any one of iron nitrate, iron chloride or iron sulfate, or a combination of at least two thereof, typical but non-limiting combinations include a combination of iron nitrate and iron chloride, a combination of iron chloride and iron sulfate, a combination of iron nitrate and iron sulfate, or a combination of iron nitrate, iron chloride and iron sulfate.

[0085] Exemplarily, the second metal oxide precursor is a metal salt corresponding to the same metal; for example, when the second metal oxide is cerium oxide, its corresponding second metal oxide precursor includes any one of cerium nitrate, cerium chloride or cerium sulfate, or a combination of at least two of them, typical but non-limiting combinations include a combination of cerium nitrate and cerium chloride, a combination of cerium chloride and cerium sulfate, a combination of cerium nitrate and cerium sulfate, or a combination of cerium nitrate, cerium chloride and cerium sulfate.

[0086] The present invention converts the first metal salt and the second metal salt in the clay-based catalyst into the first metal oxide and the second metal oxide through calcination, and adjusts the target acidic site and basic site through a sufficient calcination process.

[0087] The calcination needs to be carried out at a suitable temperature and time to obtain sufficient first metal oxide and second metal oxide, and then obtain the modification effect of the target acid-base site. Within the range given by the present invention, it is found that under the same calcination time, the higher the temperature or the longer the time at the same temperature, the more acidic sites and basic sites measured after modification. It can be seen that the improvement of acid-base sites shows a certain "time-temperature equivalence", but the increase in temperature is more significant than the extension of time; on the other hand, too high a temperature will lead to an increase in the proportion of strong acids in acidic sites, so the temperature should not be too high.

[0088] In some embodiments, the calcination temperature is 300-600°C, for example, 300°C, 350°C, 400°C, 450°C, 500°C, 550°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0089] In certain embodiments, the calcination time is 2-10 h, for example, 2 h, 3 h, 4 h, 5 h, 6 h, 8 h or 10 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0090] Within the range of calcination temperature and calcination time provided by the present invention, it is possible to achieve a basic site content of 0.8 mmol / g to 1.8 mmol / g, an acidic site content of ≤1.8 mmol / g, and an acidic site content of more than 0.9 times the basic site content. However, at the selected calcination temperature, the corresponding calcination time should be selected according to the growth of the acid and base sites to achieve sufficient calcination.

[0091] The present invention converts the first metal element in the clay-based catalyst into a first metal oxide and the second metal element into a second metal oxide by calcination. Therefore, the calcination in the present invention is carried out in an air atmosphere and / or an oxygen atmosphere.

[0092] In certain embodiments, the binder includes any one of boehmite, pseudo-boehmite, silica sol or alumina sol, or a combination of at least two of them. Typical but non-limiting combinations include a combination of boehmite and pseudo-boehmite, a combination of silica sol and alumina sol, a combination of pseudo-boehmite and alumina sol, a combination of boehmite, pseudo-boehmite and silica sol, or a combination of boehmite, pseudo-boehmite, silica sol and alumina sol.

[0093] A certain embodiment of the present invention provides use of the clay-based catalyst described in certain embodiments, wherein the clay-based catalyst is used to catalyze the synthesis of polytetrahydrofuran.

[0094] In a specific embodiment of the present invention, the test method for the acid site content in the clay-based catalyst includes an NH3-TPD test, and the test process includes: taking 100 mg of a clay-based catalyst with an average particle size of 40 mesh, placing it in a helium carrier gas environment of 30 mL / min; first heating to 300°C at a rate of 10°C / min, keeping the temperature constant for 30 minutes, and naturally cooling to 50°C. This step can remove water and other pollutants; then passing an ammonia-helium mixed gas containing 10 vol% NH3, at which time, the acid sites on the sample to be tested will chemically combine with ammonia, and after 30 minutes of adsorption, all acid sites will react with ammonia; then, purge with helium to remove the unreacted ammonia; after purging, heat to 700°C at a rate of 20°C / min for desorption. During the heating process, the NH3 adsorbed on the acid sites will gradually detach.

[0095] The chemical bond between the acidic site and ammonia is stable at 50°C. Generally, when it reaches above 100°C, the chemical bond between the acidic site and ammonia becomes unstable. The least stable one will desorb first to form a desorption peak. As the temperature continues to rise, the chemical bond with better stability will gradually desorb until all acidic sites are separated from ammonia at 700°C. Therefore, the temperature is raised to 700°C at a rate of 20°C / min to desorb ammonia, and the NH3-TPD spectrum is detected. The signal acquisition of the NH3-TPD test process uses a thermal conductivity cell detector (TPD). The detector can use the difference in thermal conductivity between the carrier gas and the gas to be tested to reflect the concentration change of ammonia during the heating process, and convert this chemical signal into a voltage signal and feed it back to the spectrum. The horizontal axis of the spectrum is temperature °C, and the vertical axis is voltage mv.

[0096] By introducing a specified amount of ammonia in advance, the corresponding relationship between the ammonia content and the integrated area of ​​the desorption peak in the spectrum can be constructed. According to the ratio that 1 mol of acid sites can adsorb 1 mol of ammonia, the ammonia adsorption amount can be converted to the acid site content. At this point, the peak area data can be converted to the acid site content data.

[0097] The stronger the acid sites, the more stable they are in combination with NH3, and the higher the temperature required for desorption. Among them, the acid sites with a peak intensity below 400°C are weak acid sites, and the acid sites with a peak intensity exceeding 400°C are strong acid sites.

[0098] In a specific embodiment of the present invention, the principle of the test method for the content of basic sites in the clay-based catalyst is consistent with the principle of the test for the content of acidic sites, and the CO2-TPD test is adopted, and the test process includes: taking 100 mg of a clay-based catalyst with an average particle size of 40 mesh, and placing it in a helium carrier gas environment of 30 mL / min; firstly heating to 300°C at a rate of 10°C / min, keeping the temperature constant for 30 minutes, and naturally cooling to 50°C; then introducing a carbon dioxide / helium mixture containing 10 vol% CO2, at which time, the basic sites on the sample to be tested will chemically combine with CO2, and after 30 minutes of adsorption, all the basic sites will react with CO2; then, helium is used to purge to remove the unreacted CO2; thereafter, the temperature is raised to 700°C at a rate of 20°C / min to desorb CO2, and a CO2-TPD spectrum is obtained by detection.

[0099] In a specific embodiment of the present invention, a test method for evaluating the blockage of macromolecules by TGA is used: the catalyst collected in the tenth application is washed three times with pure tetrahydrofuran (THF) to remove the adsorbed products on the outer surface; then, the catalyst is rotary evaporated at 150°C and 10mbar for 10 minutes to remove the volatile components with small molecular weight, and then the clay-based catalyst is removed, 100 mg is weighed, and a thermogravimetric analysis (TGA) test is performed in an air atmosphere, and the weight loss ratio in the temperature range of 200-400°C during the TGA test is recorded; the TGA used in this embodiment is the Q500 of TA Company of the United States, the supporting software version is Advantage v5.5.24, the operating mode is selected as Hi-res-Dynamic, the temperature program is 50°C / min from room temperature to 600°C, the resolution (Resolution) is 8, and the sensitivity value (Sensitivity value) is 1.

[0100] When the present invention tests the macromolecular blockage, the temperature range of 200°C to 400°C is selected because the polymer begins to decompose at around 200°C and is almost completely decomposed at 400°C, and this temperature does not reach the decomposition temperature of the catalyst. Therefore, the weight loss in this temperature range comes from the polymer residues that are difficult to wash and not easy to volatilize.

[0101] In order to clearly illustrate the technical solution of the present invention, in the following specific implementation, the binder is boehmite, cas: 1318-23-6;

[0102] In the following specific embodiments, the clay matrix of Examples 1-1 to 1-5, Comparative Examples 1 and 2 is acidified kaolin (Longyan Kaolin Co., Ltd., grade 325 mesh kaolin concentrate, the raw material is calcined at 700°C for 12h, hydrochloric acid is added, and the raw material is treated at 95°C for 12h, separated, washed and dried to obtain acidified kaolin), the initial conversion rate Y0 of the acidified kaolin is 25.9%, and the initial specific surface area is 163.5m 2 / g, pore size 3.02nm, pore volume 0.27mL / g, acid site content 0.67mmol / g, base site content 0.55mmol / g, and weak acid site content / strong acid site content 0.42;

[0103] In the following specific implementation manner, the clay matrix of Examples 2-1 to 2-6 and Comparative Examples 3 to 7 is acidified montmorillonite (Guangzhou Jingwei Mining Technology Co., Ltd., brand is high white montmorillonite, the raw material is mixed with 10wt% nitric acid, stirred and reacted at 85°C for 10h, washed and separated, and then dried to obtain acidified montmorillonite), the initial conversion rate Y0 is 25%, the initial specific surface area is 150m 2 / g, pore size 3.17nm, pore volume 0.25mL / g, acid site content 0.6mmol / g, base site content 0.5mmol / g, and weak acid site content / strong acid site content 0.4;

[0104] In the following specific implementation manner, the clay matrix of Example 3 is acidified attapulgite (Yiao New Material Technology Co., Ltd., brand attapulgite, the raw material is mixed with 4wt% sulfuric acid, stirred at 90°C for 24h, sieved, washed and separated, and the solid was dried to obtain acidified attapulgite), the initial conversion rate Y0 of the acidified attapulgite is 28.2%, and the initial specific surface area is 179.2m 2 / g, pore size 3.21nm, pore volume 0.31mL / g, acid site content 0.45mmol / g, base site content 0.62mmol / g, and weak acid site content / strong acid site content 0.51;

[0105] In the following specific implementation manner, the clay matrix of Example 4 is a compound of acidified kaolin (Longyan Kaolin Co., Ltd., brand 325 mesh kaolin concentrate, the raw material is calcined at 700°C for 12h, hydrochloric acid is added, and it is treated at 95°C for 12h, separated, washed and dried to obtain acidified kaolin) and acidified halloysite (Shijiazhuang Chenjin Mineral Products Co., Ltd., brand halloysite, the raw material is treated at 90°C for 16h in 8wt% sulfuric acid solution, separated, washed and dried to obtain acidified halloysite), the mass ratio of the compound is 4:6, the initial conversion rate Y0 of the mixed clay is 27.5%, and the initial specific surface area is 162m 2 / g, pore size 3.31nm, pore volume 0.39mL / g, acid site content 0.41mmol / g, base site content 0.58mmol / g, and weak acid site content / strong acid site content 0.46;

[0106] The total mass of the first metal oxide and the second metal oxide is less than 13 wt % of the clay-based catalyst.

[0107] The above description of the clay matrix and the adhesive is not considered as a further limitation of the technical solution of the present invention.

[0108] The upper limit of the total solute molar concentration of the mixed metal salt solution (the percentage of the total molar amount of metal salts to the mass of the solution) is to ensure that the metal salts are completely dissolved, and the lower limit is to ensure that the slurry composed of the added mixed metal salt solution, the clay matrix and the binder can be kneaded and formed and the content of the mixed metal salt reaches the target value.

[0109] Example 1-1

[0110] This embodiment provides a clay-based catalyst, which includes a clay matrix, a first metal oxide and a second metal oxide;

[0111] The first metal oxide is iron oxide, and its content is 5wt% of the clay-based catalyst;

[0112] The second metal oxide is lanthanum oxide, and its content is 5wt% of the clay-based catalyst.

[0113] The preparation method of the clay-based catalyst described in this embodiment comprises the following steps:

[0114] The clay matrix, the binder and the mixed metal salt solution are mixed according to the formula, and then the obtained slurry is kneaded into a blank, and the kneading process promotes the full mixing of the mixed metal salt solution and the clay matrix; the obtained blank is calcined at 450° C. for 6 hours in an air atmosphere to obtain the clay-based catalyst;

[0115] The binder is 15wt% of the clay matrix;

[0116] The mixed metal salt solution is a mixed solution of ferric nitrate and lanthanum nitrate.

[0117] The clay-based catalyst obtained in this example has a basic site content of 1.54 mmol / g, an acidic site content of 1.55 mmol / g, the acidic site content is 1.01 times the basic site content, and a ratio of the weak acid site content to the strong acid site content of 0.95.

[0118] In Examples 1-2 to 1-5 and Comparative Examples 1 and 2, except for the calcination temperature and calcination time, the rest are the same as Example 1-1. Table 1 discloses the calcination temperature and calcination time of the preparation process of the clay-based catalyst described in Examples 1-2 to 1-5 and Comparative Examples 1 and 2.

[0119] The basic site content of the clay-based catalyst obtained in Example 1-2 was 1.8 mmol / g, the acidic site content was 1.7 mmol / g, the acidic site content was 0.94 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 0.72, and the specific surface area was 181.2 m 2 / g, the pore diameter is 3.75nm, and the pore volume is 0.36mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 53.2%, the conversion rate Y2 is 52.1%, and the TGA weight loss ratio is 0.05%.

[0120] The basic site content of the clay-based catalyst obtained in Example 1-3 was 1.64 mmol / g, the acidic site content was 1.62 mmol / g, the acidic site content was 0.99 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 0.88, and the specific surface area was 189.4 m 2 / g, the pore diameter is 3.88nm, and the pore volume is 0.39mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 57.9%, the conversion rate Y2 is 56.2%, and the TGA weight loss ratio is 0.07%.

[0121] The basic site content of the clay-based catalyst obtained in Example 1-4 was 1.41 mmol / g, the acidic site content was 1.36 mmol / g, the acidic site content was 0.96 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.05, and the specific surface area was 200.5 m 2 / g, the pore diameter is 4.12nm, and the pore volume is 0.44mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 57.5%, the conversion rate Y2 is 55%, and the TGA weight loss ratio is 0.09%.

[0122] The basic site content of the clay-based catalyst obtained in Example 1-5 was 1.31 mmol / g, the acidic site content was 1.22 mmol / g, the acidic site content was 0.93 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.11, and the specific surface area was 208 m 2 / g, the pore diameter is 4.23nm, and the pore volume is 0.45mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 53.8%, the conversion rate Y2 is 50.4%, and the TGA weight loss ratio is 0.12%.

[0123] The basic site content of the clay-based catalyst obtained in Comparative Example 1 was 1.25 mmol / g, the acidic site content was 1.08 mmol / g, the acidic site content was 0.86 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.22, and the specific surface area was 212.7 m 2 / g, the pore diameter is 4.28nm, and the pore volume is 0.46mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 44.2%, the conversion rate Y2 is 39.9%, and the TGA weight loss ratio is 0.15%.

[0124] The basic site content of the clay-based catalyst obtained in Comparative Example 2 was 1.27 mmol / g, the acidic site content was 1.11 mmol / g, the acidic site content was 0.87 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.15, and the specific surface area was 209.5 m 2 / g, the pore diameter is 4.25nm, and the pore volume is 0.45mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 44.6%, the conversion rate Y2 is 40.2%, and the TGA weight loss ratio is 0.16%.

[0125] By comparing Examples 1-5 and Comparative Examples 1-2, it can be seen that when the calcination temperature and the calcination time change, the full formation of the first metal oxide and the second metal oxide is affected, thereby affecting the basic site content, the acidic site content, and the ratio of the weak acid site to the strong acid site content.

[0126] When the calcination temperature and calcination time are adjusted so that the basic site content is between 0.8 and 1.8 mmol / L, the acidic site content is ≤1.8 mmol / L and the acidic site content is more than 0.9 times the basic site content, the obtained clay-based catalyst has a good first conversion rate and a conversion rate after the tenth application, and the TGA weight loss ratio is low.

[0127] From the comparison of Comparative Examples 1 and 2 with Example 1-1, it can be seen that when the basic site content is between 0.8 and 1.8 mmol / L and the acidic site content is ≤1.8 mmol / L, but the acidic site content is less than 0.9 times the basic site content, the first conversion rate is significantly reduced.

[0128] Therefore, in order to make the obtained clay-based catalyst have good catalytic performance when catalyzing the synthesis of polytetrahydrofuran, it is necessary to make the basic site content between 0.8 and 1.8 mmol / L, the acidic site content ≤ 1.8 mmol / L and the acidic site content more than 0.9 times the basic site content.

[0129] Table 1

[0130]

[0131] Example 2-1

[0132] This embodiment provides a clay-based catalyst, which includes a clay matrix, a first metal oxide and a second metal oxide;

[0133] The first metal oxide is zirconium oxide and copper oxide in a mass ratio of 2:1, and its content is 6wt% of the clay-based catalyst;

[0134] The second metal oxide is yttrium oxide, and its content is 4 wt % of the clay-based catalyst.

[0135] The preparation method of the clay-based catalyst described in this embodiment comprises the following steps:

[0136] The clay matrix, the binder and the mixed metal salt solution are mixed according to the formula, and then the obtained slurry is kneaded into a blank, and the kneading process promotes the full mixing of the mixed metal salt solution and the clay matrix; the obtained blank is calcined at 500° C. for 5 hours in an oxygen atmosphere to obtain the clay-based catalyst;

[0137] The binder is 10wt% of the clay matrix;

[0138] The mixed metal salt solution is a mixed solution of zirconium sulfate, copper sulfate and yttrium nitrate.

[0139] The clay-based catalyst obtained in this example has a basic site content of 1.13 mmol / g and an acidic site content of 1.50 mmol / g. The acidic site content is 1.33 times that of the basic site content, and the ratio of the weak acidic site content to the strong acidic site content is 0.92.

[0140] In Examples 2-2 to 2-6, except that the first metal oxide and the second metal oxide are changed as shown in Table 2, the rest are the same as Example 2-1.

[0141] The basic site content of the clay-based catalyst obtained in Example 2-2 was 1.01 mmol / g, the acidic site content was 1.05 mmol / g, the acidic site content was 1.04 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.33, and the specific surface area was 228.2 m 2 / g, the pore diameter is 3.94nm, and the pore volume is 0.3mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 58.4%, the conversion rate Y2 is 53.1%, and the TGA weight loss ratio is 0.26%.

[0142] The basic site content of the clay-based catalyst obtained in Example 2-3 was 1.45 mmol / g, the acidic site content was 1.33 mmol / g, the acidic site content was 0.92 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.51, and the specific surface area was 185.8 m 2 / g, the pore diameter is 4.13nm, and the pore volume is 0.4mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 51.9%, the conversion rate Y2 is 49.6%, and the TGA weight loss ratio is 0.08%.

[0143] The basic site content of the clay-based catalyst obtained in Example 2-4 was 0.82 mmol / g, the acidic site content was 1.27 mmol / g, the acidic site content was 1.55 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.96, and the specific surface area was 212.2 m 2 / g, the pore diameter is 4.48nm, and the pore volume is 0.43mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 61.4%, the conversion rate Y2 is 54.3%, and the TGA weight loss ratio is 0.28%.

[0144] The basic site content of the clay-based catalyst obtained in Example 2-5 was 0.99 mmol / g, the acidic site content was 0.99 mmol / g, the acidic site content was 1 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.29, and the specific surface area was 185.1 m 2 / g, the pore diameter is 4.24nm, and the pore volume is 0.38mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 56.5%, the conversion rate Y2 is 49.1%, and the TGA weight loss ratio is 0.27%.

[0145] The basic site content of the clay-based catalyst obtained in Example 2-6 was 1.1 mmol / g, the acidic site content was 1.46 mmol / g, the acidic site content was 1.33 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 0.68, and the specific surface area was 161.1 m 2 / g, the pore diameter is 4.35nm, and the pore volume is 0.35mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 55.8%, the conversion rate Y2 is 48%, and the TGA weight loss ratio is 0.3%.

[0146] It can be seen from Examples 2-1 to 2-6 that adjusting the type and content of the first metal oxide and the second metal oxide will affect the content of basic sites, the content of acidic sites, and the ratio of the content of weak acidic sites to that of strong acidic sites.

[0147] When the calcination temperature and calcination time are adjusted so that the basic site content is between 0.8 and 1.8 mmol / L, the acidic site content is ≤1.8 mmol / L and the acidic site content is more than 0.9 times the basic site content, the obtained clay-based catalyst has a good first conversion rate and a conversion rate after the tenth application, and the TGA weight loss ratio is low.

[0148] From the comparison between Example 2-6 and Example 2-1, it can be seen that when the basic site content is required to be 0.8-1.8 mmol / L, the acid site content is ≤1.8 mmol / L and the acid site content is more than 0.9 times the basic site content, the effect of inhibiting macromolecular blockage is better when the ratio of the weak acid site content to the strong acid site content is controlled within the range of 0.7-2. Compared with Example 2-6, when the ratio of the weak acid to strong acid site content in Example 2-1 is increased to 0.92, the TGA weight loss ratio is reduced, and the specific surface area of ​​the obtained clay-based catalyst is significantly increased.

[0149] Table 2

[0150]

[0151]

[0152] In the preparation methods of the clay-based catalysts of Comparative Examples 3 to 7, except for adjusting the components of the salt solution so that the first metal oxide and the second metal oxide obtained after calcination change as shown in Table 3, the rest are the same as Example 2-1.

[0153] The basic site content of the clay-based catalyst obtained in Comparative Example 3 is 0.97 mmol / g, the acidic site content is 0.83 mmol / g, the acidic site content is 0.86 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content is 0.92, and the specific surface area is 184.9 m 2 / g, the pore diameter is 3.98nm, and the pore volume is 0.29mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 42.2%, the conversion rate Y2 is 34.6%, and the TGA weight loss ratio is 0.29%.

[0154] The basic site content of the clay-based catalyst obtained in Comparative Example 4 was 1.13 mmol / g, the acidic site content was 0.97 mmol / g, the acidic site content was 0.86 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 0.9, and the specific surface area was 202.5 m 2 / g, the pore diameter is 4.21nm, and the pore volume is 0.33mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 41.9%, the conversion rate Y2 is 37.2%, and the TGA weight loss ratio is 0.22%.

[0155] The basic site content of the clay-based catalyst obtained in Comparative Example 5 is 0.77 mmol / g, the acidic site content is 1.03 mmol / g, the acidic site content is 1.34 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content is 1.04, and the specific surface area is 232.1 m 2 / g, the pore diameter is 4.06nm, and the pore volume is 0.31mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 58.4%, the conversion rate Y2 is 41.6%, and the TGA weight loss ratio is 0.56%.

[0156] The basic site content of the clay-based catalyst obtained in Comparative Example 6 is 0.72 mmol / g, the acidic site content is 1.5 mmol / g, the acidic site content is 2.08 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content is 0.74, and the specific surface area is 226.2 m 2 / g, the pore diameter is 4.2nm, and the pore volume is 0.31mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 65.3%, the conversion rate Y2 is 38.9%, and the TGA weight loss ratio is 0.88%.

[0157] The basic site content of the clay-based catalyst obtained in Comparative Example 7 was 1.1 mmol / g, the acidic site content was 0.67 mmol / g, the acidic site content was 0.61 times the basic site content, the ratio of the weak acidic site content to the strong acidic site content was 1.63, and the specific surface area was 232.3 m 2 / g, the pore diameter is 4.35nm, and the pore volume is 0.35mL / g; the catalytic effect data of the clay-based catalyst obtained in this comparative example are evaluated, the conversion rate Y1 is 36.1%, the conversion rate Y2 is 30.9%, and the TGA weight loss ratio is 0.21%.

[0158] Table 3

[0159]

[0160] Example 1-1 and Comparative Example 1 and Comparative Example 2 are a set of comparative experiments. It can be seen from the comparison that insufficient calcination will affect the acquisition of the target acid-base sites, especially the increase in the acid site content, which will lead to a low initial conversion rate of the catalyst when catalyzing the THF polymerization reaction. Therefore, when preparing the catalyst, the calcination process should be adaptively adjusted according to the target value of the acid-base site.

[0161] Example 2-1 and Comparative Example 4 are a set of comparative experiments. By comparison, it can be seen that under the same base site concentration, a too small acid-base site ratio will lead to poor conversion rate.

[0162] Example 2-1 and Comparative Example 5 are a set of comparative experiments. The comparison shows that, under the same acid-base site ratio, too few basic sites will not be effective in inhibiting excessively long molecular chains.

[0163] Too small a ratio of acidic and basic sites will result in poor conversion rate, while too few basic sites will result in poor effect in suppressing the production of overly long molecular chains.

[0164] Example 2-1 and Comparative Examples 3, 6 and 7 form a group of comparative examples. The first metal and the second metal have different contributions to the regulation of acid-base sites, and the types and ratios of the first metal and the second metal need to be adaptively matched according to the target values ​​of the acid-base sites.

[0165] Example 3

[0166] This embodiment provides a clay-based catalyst, which includes a clay matrix, a first metal oxide and a second metal oxide;

[0167] The first metal oxide is iron oxide, and its content is 4wt% of the clay-based catalyst;

[0168] The second metal oxide is lanthanum oxide, and its content is 3 wt % of the clay-based catalyst.

[0169] The preparation method of the clay-based catalyst described in this embodiment comprises the following steps:

[0170] The clay matrix, the binder and the mixed metal salt solution are mixed according to the formula, and then the obtained slurry is kneaded into a blank, and the kneading process promotes the full mixing of the mixed metal salt solution and the clay matrix; the obtained blank is calcined at 500° C. for 4 hours in an air atmosphere to obtain the clay-based catalyst;

[0171] The binder is 9.5wt% of the clay matrix;

[0172] The mixed metal salt solution is a mixed solution of ferric nitrate and lanthanum nitrate.

[0173] The clay-based catalyst obtained in this example has a basic site content of 1.21 mmol / g and an acidic site content of 1.55 mmol / g. The acidic site content is 1.28 times the basic site content. The ratio of the weak acidic site content to the strong acidic site content is 1.01. The specific surface area is 303.9 m 2 / g, the pore diameter is 4.29nm, and the pore volume is 0.36mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 65.2%, the conversion rate Y2 is 60.8%, and the TGA weight loss ratio is 0.07%.

[0174] Example 4

[0175] This embodiment provides a clay-based catalyst, which includes a clay matrix, a first metal oxide and a second metal oxide;

[0176] The first metal oxide is zinc oxide, and its content is 6.5wt% of the clay-based catalyst;

[0177] The second metal oxide is lanthanum oxide, and its content is 3.2 wt % of the clay-based catalyst.

[0178] The preparation method of the clay-based catalyst described in this embodiment comprises the following steps:

[0179] The clay matrix, the binder and the mixed metal salt solution are mixed according to the formula, and then the obtained slurry is kneaded into a blank, and the kneading process promotes the full mixing of the mixed metal salt solution and the clay matrix; the obtained blank is calcined at 450° C. for 5 hours in an air atmosphere to obtain the clay-based catalyst;

[0180] The binder is 12wt% of the clay matrix;

[0181] The mixed metal salt solution is a mixed solution of zinc nitrate and lanthanum nitrate.

[0182] The clay-based catalyst obtained in this example has a basic site content of 1.39 mmol / g and an acidic site content of 1.43 mmol / g. The acidic site content is 1.03 times the basic site content. The ratio of the weak acidic site content to the strong acidic site content is 1.08. The specific surface area is 244.5 m 2 / g, the pore diameter is 4.21nm, and the pore volume is 0.47mL / g; the catalytic effect data of the clay-based catalyst obtained in this example are evaluated, the conversion rate Y1 is 58.5%, the conversion rate Y2 is 55.9%, and the TGA weight loss ratio is 0.11%.

[0183] In summary, during the polymerization reaction, the alkaline site does not catalyze the chain growth reaction, but the alkaline site is easy to combine with water, resulting in an increase in the water content near the clay-based catalyst. The prior art usually reduces the content of the alkaline site to reduce the adverse effect of the alkaline site on the catalytic activity. The present invention utilizes the characteristic that the inhibitory effect of the alkaline site on the growth of the polymer chain is greater than the inhibitory effect on the growth of the low molecular weight chain, increases the content of the alkaline site in the clay-based catalyst, and simultaneously increases the content ratio of the acidic site to the alkaline site, so that the catalytic activity gain brought by the overall increase in the acidic site content exceeds the loss effect brought by the increase in the alkaline site, and retains the inhibitory effect of the increase in the alkaline site on the macromolecular chain, which can reduce the catalyst pore blockage caused by the production of macromolecules while ensuring the conversion rate, thereby ensuring the catalytic activity.

[0184] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.

Claims

1. A clay-based catalyst, characterized in that: The basic site content in the clay-based catalyst is 0.8 mmol / g to 1.8 mmol / g; The acidic site content in the clay-based catalyst is ≤1.8 mmol / g; The acidic site content is 0.9 times or more of the basic site content.

2. The clay-based catalyst according to claim 1, characterized in that The acid sites include strong acid sites and weak acid sites; The ratio of the content of the weak acid sites to the content of the strong acid sites is 0.7-2.

3. The clay-based catalyst according to claim 1 or 2, characterized in that: The clay-based catalyst comprises a clay matrix, a first metal oxide and a second metal oxide; The first metal oxide is an oxide capable of increasing the acid site content of the clay-based catalyst; The second metal oxide is an oxide capable of increasing the basic site content of the clay-based catalyst.

4. The clay-based catalyst according to claim 3, characterized in that The first metal oxide includes any one of iron oxide, zirconium oxide, titanium dioxide, cobalt oxide, nickel oxide, copper oxide, zinc oxide or molybdenum oxide, or a combination of at least two thereof.

5. The clay-based catalyst according to claim 3, characterized in that The second metal oxide includes any one of lanthanum oxide, cerium oxide, samarium oxide or yttrium oxide, or a combination of at least two thereof.

6. The clay-based catalyst according to claim 3, characterized in that The clay matrix includes any one of attapulgite, montmorillonite, kaolin or halloysite, or a combination of at least two of them.

7. The clay-based catalyst according to claim 3, characterized in that The clay matrix is ​​acidified clay; The specific surface area of ​​the acidified clay is ≥150m 2 / g, pore diameter ≥3nm, pore volume ≥0.25mL / g.

8. A method for preparing a clay-based catalyst according to any one of claims 1 to 7, characterized in that: The preparation method comprises the following steps: Mixing a clay matrix, a binder and a mixed metal salt solution according to a formula, and then kneading the obtained slurry into a blank; calcining the obtained blank to obtain the clay-based catalyst; The mixed metal salt solution is a solution comprising a first metal salt and a second metal salt; The first metal salt and the second metal salt are converted into the first metal oxide and the second metal oxide after calcination.

9. The preparation method according to claim 8, characterized in that: The calcination temperature is 300° C. to 600° C., and the calcination time is 2 h to 10 h.

10. A use of the clay-based catalyst according to any one of claims 1 to 7, characterized in that: The clay-based catalyst is used for catalyzing the synthesis of polytetrahydrofuran.

Citation Information

Patent Citations

  • Catalyst, method for producing the same and method for the polymerisation of cyclic ethers on said catalyst

    CN1684762A

  • Method for preparing polyether glycols

    US4127513A