Organosilicon-polyaniline copolymer self-repairing thermal interface material and preparation method thereof
By introducing polyaniline and silicone structural units on the polymer main chain and combining modified hexagonal boron nitride nanosheets to form a silicone-polyaniline copolymer thermal interface material, the thermal conductivity and self-conductivity in the prior art are solved. The contradiction between repair efficiency achieves the effects of high thermal conductivity and high self-healing.
Patent Information
- Application Number
- CN202411201266.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing filler polymer thermal interface materials are difficult to balance between high thermal conductivity and self-repair efficiency, and cannot meet the needs of the field of smart electronics, and the high solids content leads to a decrease in self-repair efficiency.
By introducing highly conductive polyaniline and silicone structural units that can hydrolyze the hydrogen bond network on the polymer main chain, a silicone-polyaniline copolymer is formed, and combined with modified hexagonal boron nitride nanosheets, a thermal conductivity network is established and Hydrogen bond network improves the thermal conductivity and self-healing performance of materials.
It achieves high thermal conductivity (up to 9.324W/(m·K) and high self-repair efficiency (94.7%), while reducing the solid content, solving the mutually exclusive problems of thermal conductivity and self-repair performance.
Smart Images

Figure CN118930865A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal interface materials, and relates to an organosilicon-polyaniline copolymer self-repairing thermal interface material and a preparation method thereof. Background Art
[0002] The rapid development of science and technology has led to the development of electronic equipment in the direction of lightweight, integration, miniaturization, and multifunctionality. The cooling space of the instrument has shrunk, and the power density has continued to increase, resulting in uneven heat flow distribution. Local overheating has seriously affected the stability and performance of the equipment. Studies have shown that the service life of electronic equipment and devices will be shortened by 50% for every 10-15℃ increase in operating temperature. Temperature control has become an urgent requirement for stable, reliable, and safe operation of equipment.
[0003] Thermal interface material is a material widely used in integrated circuit packaging and electronic heat dissipation. It is mainly used to fill the micropores and uneven holes between the heater and the heat sink, thereby eliminating the air gap to increase the effective heat conduction channel, reduce the contact thermal resistance, and improve the heat dissipation efficiency. Polymer materials have the advantages of light weight, good flexibility, outstanding processing performance, good electrical insulation and corrosion resistance, and account for more than 90% of the market share in thermal interface materials. The thermal conductivity of most polymers is concentrated in the range of 0.1 to 0.5 W / (m·K), but the minimum thermal conductivity requirement for thermal interface materials used in high-density integrated electronic devices is 1 W / (m·K).
[0004] In this field, there are two main methods commonly used to improve the thermal conductivity of polymers: one is to design the polymer chain morphology and synthesize intrinsic thermal conductive polymer materials. This method is complex and difficult to achieve large-scale production; the second is to use high thermal conductive fillers to fill the polymer matrix, such as CN118027674A, which has the advantages of low cost, simple process, and wide applicability. In addition, the polymer matrix can be given multifunctionality through the structural design of the polymer matrix or the structural design of the thermal conductive filler to meet the different needs of polymer-based thermal conductive materials in the fields of aerospace, automobiles, microelectronics, etc.
[0005] At present, most of the thermally conductive composite materials widely used in various fields are filled polymer-based thermally conductive materials. However, the current filled polymer thermal interface materials have the problems of poor heat resistance and poor adhesion. Traditional filled polymer thermal interface materials also have the disadvantages of being unable to self-repair mechanical damage or having low repair efficiency, and cannot meet the demand for materials in the field of smart electronics. At the same time, in order to improve the thermal conductivity of composite materials, a large amount of inorganic thermally conductive fillers are often added, which will reduce the content of the polymer matrix and weaken the interaction between polymer chains. Compared with the interaction of the dynamic reversible bonds of polymers, the interaction of inorganic fillers is much smaller, so high thermal conductivity and high self-repair efficiency are often mutually exclusive. Therefore, it is of great significance to develop a thermal interface material with both high thermal conductivity and high self-repair efficiency. Summary of the invention
[0006] The traditional polymer composite thermal interface material has a significant decrease in self-healing efficiency due to its high solid content, and it is difficult to obtain a polymer composite thermal conductive material with both high thermal conductivity and high self-healing efficiency. In order to solve this problem, the present application starts with the chemical structure of the polymer substrate, and introduces a highly conductive structural unit polyaniline and a siloxane that can hydrolyze a large number of hydroxyl groups to form a hydrogen bond network on the polymer main chain by copolymerization. The introduction of these two structural units can introduce a large number of free electrons into the composite material on the one hand, thereby improving the thermal conductivity of the material; in addition, the siloxane group can hydrolyze to produce a large number of silanol groups, which can provide a large number of hydrogen bond networks in the system, thereby improving the self-healing performance of the material. At the same time, the π-π stacking effect of polyaniline has an interactive force with the thermally conductive filler that also has a planar stacking effect, which is conducive to the establishment of a thermal conductive network between the polymer substrate and the thermally conductive filler, so that the thermal interface composite material has the effects of self-healing and high thermal conductivity at the same time.
[0007] In a first aspect of the present invention, a silicone-polyaniline copolymer is provided, wherein the silicone-polyaniline copolymer has the structural formula:
[0008]
[0009] Among them, POMS is pendant alkoxy polysiloxane, and PANI is polyaniline;
[0010] Among them, R1, R2, R3, R4, R7, and R8 are independently selected from one of methyl, ethyl, or propyl, and R5 and R6 are independently selected from one of methyl, ethyl, trifluoropropyl, or phenyl; m and o are independently natural numbers of 20 to 5000, and n and p are independently natural numbers of 50 to 1500.
[0011] Preferably, m is a natural number of 200 to 300, n is a natural number of 50 to 250, o is a natural number of 500 to 750, and p is a natural number of 90 to 350.
[0012] In a specific embodiment of the present invention, the m, n, o, and p satisfy: (n+p) / (m+n+o+p)*100%=5-45%, preferably 15-36%. If this value is too low, there are few silanol groups that can be hydrolyzed in the system, few hydrogen bonds are formed, the strength of the dynamic hydrogen bonds formed is very weak, and the self-healing performance is very poor. However, if it exceeds this range, it means that the content of silanol groups is too high, and the silanol groups are easily self-crosslinked. Although the mechanical strength of the system is improved, the silanol groups that can provide hydrogen bonds are reduced, and the self-healing efficiency is still very low.
[0013] In a specific embodiment of the present invention, y and z are respectively and independently natural numbers of 100 to 1500, and the value of y / (y+z) is 25 to 85%, preferably 35 to 65%, and more preferably 45 to 52%. Thus, the conductivity of the organosilicon-polyaniline copolymer is optimal.
[0014] Preferably, y is a natural number between 100 and 300, and z is a natural number between 100 and 300.
[0015] Preferably, the structural formula of the organosilicon-polyaniline copolymer is:
[0016]
[0017]
[0018] In a second aspect of the present invention, a method for preparing the above-mentioned organosilicon-polyaniline copolymer is provided, comprising the following steps:
[0019] (a) adding polyaniline to hydrogen-containing silicone oil, and then adding an organic solvent to mix well;
[0020] (b) adding tetramethylammonium hydroxide to the uniformly mixed solution, and stirring the reaction until no gas is generated;
[0021] (c) adding an acidic cation exchange resin, stirring and then filtering to obtain the organosilicon-polyaniline copolymer.
[0022] In a specific embodiment of the present invention, the organic solvent in step (a) is selected from methanol.
[0023] In a specific embodiment of the present invention, the temperature for uniform mixing in step (a) is 30 to 80°C, preferably 45 to 55°C.
[0024] In a specific embodiment of the present invention, the stirring reaction temperature in step (b) is 30 to 80°C, preferably 45 to 55°C.
[0025] In a specific embodiment of the present invention, the usage ratio of polyaniline to hydrogen-containing silicone oil in step (a) is (5.6-13.5) g: (200-450) mL.
[0026] In a specific embodiment of the present invention, the acidic cation exchange resin in step (c) is NKC-9.
[0027] In a specific embodiment of the present invention, the stirring time in step (c) is 2 to 6 hours.
[0028] In a third aspect of the present invention, a self-repairing thermal interface material of an organosilicon-polyaniline copolymer is provided. The raw materials of the self-repairing thermal interface material include: the above-mentioned organosilicon-polyaniline copolymer, isopropyl titanate and a thermally conductive filler.
[0029] In a specific embodiment of the present invention, the thermal conductive filler is modified hexagonal boron nitride nanosheets.
[0030] In a specific embodiment of the present invention, the mass fraction of the thermally conductive filler in the raw material is 25-75%. For example, the mass fraction of the thermally conductive filler in the raw material is 25%, 30%, 35%, 40%, 45%, 49%, 50%, 55%, 60%, 65%, 70% or 75%.
[0031] In a specific embodiment of the present invention, in the mixture of the organosilicon-polyaniline copolymer and isopropyl titanate, the mass fraction of the organosilicon-polyaniline copolymer is 95-98%, for example, 95%, 95.5%, 96%, 96.5%, 97%, 97.5% or 98%; the mass fraction of the isopropyl titanate is 2-5%, for example, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%.
[0032] In a specific embodiment of the present invention, the preparation process of the modified hexagonal boron nitride nanosheets comprises:
[0033] S1. Mixing boron nitride powder and nitric acid and stirring at 10-70° C. for 4-24 hours to obtain a pre-treated dispersion;
[0034] S2, adding the pretreated dispersion into a mixed solution of formic acid and sulfuric acid, stirring at 0-50°C for 1-12h to obtain a dispersion, washing with water for multiple times, neutralizing and filtering until the pH value of the filtrate is 5.0-7.5, and then drying;
[0035] S3, adding the product into a solvent to prepare a highly dispersed liquid, adding a silane coupling agent and stirring for 4 to 24 hours, ultrasonically treating for 8 to 24 hours and then centrifuging to obtain the modified hexagonal boron nitride nanosheets with a thickness of 1 to 4 nm in the supernatant.
[0036] The preparation process of the modified hexagonal boron nitride nanosheets also includes at least one of the following technical features:
[0037] In step S1, the ratio of boron nitride powder to nitric acid is 10 g: (150-300) mL;
[0038] The volume ratio of formic acid to sulfuric acid in the mixed solution of step S2 is (20:80) to (60:40);
[0039] The pH value of step S2 is preferably 5.5 to 7.0, more preferably 6.0;
[0040] The concentration of the high dispersion in step S3 is 10-45 mg / mL;
[0041] The solvent in step S3 is DMF;
[0042] The silane coupling agent in step S3 is KH550.
[0043] After modification, a large number of hydroxyl groups are formed on the surface of hexagonal boron nitride nanosheets, which can form a dynamic hydrogen bond network with the silanol groups obtained by hydrolysis of organic silicon-polyaniline copolymers.
[0044] In a fourth aspect of the present invention, a method for preparing the above-mentioned organosilicon-polyaniline copolymer self-repairing thermal interface material is provided, comprising the following steps:
[0045] (1) mixing the organosilicon-polyaniline copolymer and the thermal conductive filler, stirring under vacuum conditions, and cooling to room temperature;
[0046] (2) adding isopropyl titanate, stirring under vacuum conditions, and cooling after stirring;
[0047] (3) pouring the cooled slurry onto a release film, forming a sheet through a roller press, and obtaining the organosilicon-polyaniline copolymer self-healing thermal interface material after curing.
[0048] The preparation method of the organosilicon-polyaniline copolymer self-repairing thermal interface material also includes at least one of the following technical features:
[0049] The cooling in step (2) refers to cooling with ice water at 0 to 8°C;
[0050] The stirring time under vacuum conditions in step (1) and step (2) is 30 to 180 seconds.
[0051] Beneficial effects:
[0052] (1) The organosilicon-polyaniline copolymer in the self-healing thermal interface material of the present invention has an organosilicon macromolecule as the main chain. A large number of alkoxy groups on the side groups of the organosilicon molecular chain become silanol groups after hydrolysis. The silanol groups can form a dynamic hydrogen bond network with the hydroxyl ligands on the surface of the modified hexagonal boron nitride, thereby tightly combining the organosilicon molecular chain and the thermally conductive filler; polyaniline is a conductive structural unit, and its electronic thermal conductivity can further accelerate the heat transfer of the polymer. The thermal conductivity of electrons is usually high, so the electrons in the conductive material can effectively transfer heat, thereby improving the thermal conductivity of the composite material. At the same time, the planar stacking effect of the benzene rings of polyaniline can combine with the hexagonal boron nitride nanosheets with the same planar structure to produce a good interaction force, further promoting the construction of a thermal network between the polymer and the thermally conductive filler, and solving the thermal conduction loss between the phase interfaces caused by the difference in thermal conductivity between the polymer and the thermally conductive filler;
[0053] (2) The present invention combines two polymer monomers with a self-healing hydrogen bond network and high electronic thermal conductivity, and simultaneously improves the self-healing performance and thermal conductivity of the polymer substrate through a copolymer method;
[0054] (3) The self-repairing thermal interface material of the present invention has a high thermal conductivity (the thermal conductivity can reach up to 9.324W / (m·K)), and the mechanical self-repairing efficiency can reach 94.7%;
[0055] (4) The modified boron nitride has a smaller nanosize and is easier to form a thermal conductive network. Therefore, compared with the prior art, the self-healing thermal interface material provided by the present invention has a lower solid content and a higher self-healing efficiency. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 The microscopic morphology of the modified hexagonal boron nitride nanosheets prepared in Example 1 of the present invention (left) and the microscopic morphology of the cross section of the self-healing thermal interface material (right)
[0057] Figure 2 The mechanical properties test results of the self-repairing thermal interface material prepared in Example 1 of the present invention are shown in FIG.
[0058] Figure 3 Schematic diagram of the self-repairing mechanism of the self-repairing thermal interface material prepared in Example 1 of the present invention
[0059] Figure 4 Optical photos of the self-repairing thermal interface material prepared in Example 1 of the present invention before and after self-repairing
[0060] Figure 5The thermal conductivity of the self-repairing thermal interface material prepared in Example 1 of the present invention is in its original state and after self-repairing once and twice. DETAILED DESCRIPTION
[0061] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0062] The present invention provides a self-repairing thermal interface material of an organosilicon-polyaniline copolymer and a preparation method thereof. The preparation method comprises three steps of synthesizing the organosilicon-polyaniline copolymer, preparing modified hexagonal boron nitride nanosheets, and preparing the self-repairing thermal interface material, specifically:
[0063] Step 1: Synthesis of silicone-polyaniline copolymer
[0064] Mix octadecyl ammonium polyoxyethylene ether (PEGO) and aniline (ANI) at -10 to 10°C and stir evenly;
[0065] Add ammonium persulfate, carry out polymerization reaction at -10 to 10°C for 3 to 24 hours, and then pour out the product. Preferably, the polymerization reaction temperature is 0 to 5°C;
[0066] The product is filtered and washed repeatedly with pure water for 3 to 6 times to obtain polyaniline polymer (PANI);
[0067] Add PANI to hydrogenated silicone oil, then add methanol solution and heat to 30-80°C and stir evenly, preferably at 45-55°C;
[0068] Tetramethylammonium hydroxide is added dropwise and stirred at 30-80°C until no gas is generated, preferably at 45-55°C;
[0069] Acidic cation exchange resin is added and stirred for 2 to 6 hours; the product is filtered and distilled to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)).
[0070] Step 2: Preparation of modified hexagonal boron nitride nanosheets
[0071] Pour the boron nitride powder into nitric acid and stir at a temperature of 10 to 70° C. for 4 to 24 hours to obtain a pre-treated dispersion;
[0072] The pre-treated dispersion is poured into a mixed solution of formic acid and sulfuric acid, stirred at 0-50°C for 1-12 hours to obtain a dispersion, washed with water for multiple times, neutralized and filtered until the pH value of the filtrate is about 6.5, and then dried;
[0073] The dried product is added to a DMF solvent to prepare a highly dispersed liquid, and an aqueous solution of KH550 is added and stirred for 4 to 24 hours. After ultrasonic treatment for 8 to 24 hours, the mixture is centrifuged and separated to obtain modified hexagonal boron nitride nanosheets with a thickness of 1 to 4 nm in the supernatant.
[0074] in:
[0075] The dosage ratio of the boron nitride powder to nitric acid is 10 g: (150-300) mL;
[0076] The volume ratio of formic acid to sulfuric acid in the mixed solution of formic acid and sulfuric acid is (20:80) to (60:40);
[0077] The concentration of the high dispersion liquid is 10-45 mg / mL.
[0078] Step 3: Preparation of self-repairing thermal interface material
[0079] The P(OMS-ANI) prepared in step 1 and the modified hexagonal boron nitride nanosheets prepared in step 2 are uniformly mixed, stirred for 30 to 180 seconds under vacuum conditions, and cooled to room temperature;
[0080] Add isopropyl titanate, stir for 30 to 180 seconds under vacuum, and cool after stirring; the cooling is cooling with 0 to 8° C. ice water;
[0081] The cooled slurry is poured onto a release film, formed into sheets by a roller press, and placed in the air for automatic curing for 48 hours to obtain the final product, a self-repairing thermal interface material.
[0082] In a specific embodiment of the present invention, the hydrogen-containing silicone oil is purchased from Wacker Chemical Company with a model number of TSF484.
[0083] The present invention is further described in detail below through specific embodiments.
[0084] Example 1
[0085] (1) Mix 1.5 g of octadecyl ammonium polyoxyethylene ether (PEGO) and 2.5 g of aniline (ANI) at 0°C and stir until uniform;
[0086] (2) adding 2.3 g of ammonium persulfate, carrying out polymerization reaction at 0° C. for 12 h, and then pouring out the product;
[0087] (3) The product was filtered and washed with pure water for 4 times to obtain polyaniline polymer (PANI);
[0088] (4) Add 8.5 g of PANI to 250 mL of hydrogenated silicone oil, add 300 mL of methanol solution, heat to 50 °C and stir evenly;
[0089] (5) Add 0.15 g of tetramethylammonium hydroxide dropwise and stir at 50° C. until no more gas is generated;
[0090] (6) Add 2.5 g of acidic cation exchange resin (NKC-9) and stir for 2 h; filter and distill the product to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)), the structural formula of which is:
[0091]
[0092] (7) Pour 10 g of boron nitride powder into 250 mL of nitric acid and stir at 50 °C for 12 h to obtain a pretreated dispersion;
[0093] (8) pouring the pretreated dispersion into a mixed solution of formic acid and sulfuric acid (volume ratio of 40:60) and stirring at 10° C. for 8 h to obtain a dispersion, washing with water for multiple times and filtering until the pH value of the filtrate is 5.5, and then drying;
[0094] (9) adding the product of step (8) into DMF solvent to prepare a 25 mg / mL high dispersion, adding an aqueous solution of KH550 and stirring for 12 h, ultrasonically treating for 10 h and then centrifuging to obtain a modified hexagonal boron nitride nanosheet with a thickness of 3 nm in the supernatant;
[0095] (10) 30 g of P(OMS-ANI) was added to a stirring container, followed by 29.1 g of thermally conductive filler-modified hexagonal boron nitride nanosheets, and the mixture was stirred in a blender for 120 s and then stirred under vacuum for 60 s.
[0096] (11) Place the mixture in cold water and cool it to room temperature, then add 0.9 g of isopropyl titanate, stir for 120 s under vacuum, and then place the mixture in ice water and cool it;
[0097] (12) Pour the cooled slurry onto a release film, form it into sheets through a roller press, and after curing, obtain a self-repairing thermal interface material with a thermal conductive filler mass fraction of 49%.
[0098] Example 2
[0099] (1) Mix 2.5 g of octadecyl ammonium polyoxyethylene ether (PEGO) and 1.8 g of aniline (ANI) at 5°C and stir until uniform;
[0100] (2) adding 2.2 g of ammonium persulfate, carrying out polymerization reaction at 5° C. for 10 h, and then pouring out the product;
[0101] (3) The product was filtered and washed with pure water for three times to obtain polyaniline polymer (PANI);
[0102] (4) Add 6.5 g of PANI to 250 mL of hydrogenated silicone oil, add 350 mL of methanol solution, heat to 50 °C and stir evenly;
[0103] (5) Add 0.20 g of tetramethylammonium hydroxide dropwise and stir at 50° C. until no more gas is generated;
[0104] (6) Add 5.5 g of acidic cation exchange resin (NKC-9) and stir for 2 h; filter and distill the product to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)), the structural formula of which is:
[0105]
[0106] (7) Pour 10 g of boron nitride powder into 350 mL of nitric acid and stir at 50 °C for 18 h to obtain a pretreated dispersion;
[0107] (8) The pretreated dispersion was poured into a mixed solution of formic acid and sulfuric acid (volume ratio of 40:60) and stirred at 10°C for 8 h to obtain a dispersion, which was then washed with water for multiple times and filtered until the pH value of the filtrate was 5.5 and then dried;
[0108] (9) adding the product of step (8) into DMF solvent to prepare a 25 mg / mL high dispersion, adding an aqueous solution of KH550 and stirring for 12 h, ultrasonically treating for 10 h and then centrifuging to obtain a modified hexagonal boron nitride nanosheet with a thickness of 3 nm in the supernatant;
[0109] (10) 30 g of P(OMS-ANI) was added to a stirring container, followed by 29.1 g of thermally conductive filler-modified hexagonal boron nitride nanosheets, and the mixture was stirred in a blender for 120 s and then stirred under vacuum for 60 s.
[0110] (11) Place the mixture in cold water and cool to room temperature, add 0.9 g of isopropyl titanate, stir for 120 s under vacuum, and then place the mixture in ice water and cool;
[0111] (12) Pour the cooled slurry onto a release film, form it into sheets through a roller press, and after curing, obtain a self-repairing thermal interface material with a thermal conductive filler mass fraction of 49%.
[0112] Example 3
[0113] (1) Mix 2.0 g of octadecyl ammonium polyoxyethylene ether (PEGO) and 2.4 g of aniline (ANI) at 10° C. and stir until uniform;
[0114] (2) adding 1.7 g of ammonium persulfate, carrying out polymerization reaction at 10° C. for 8 h, and then pouring out the product;
[0115] (3) The product was filtered and washed with pure water for 5 times to obtain polyaniline polymer (PANI);
[0116] (4) Add 4.5 g of PANI to 500 mL of hydrogenated silicone oil, add 450 mL of methanol solution, heat to 55 °C and stir evenly;
[0117] (5) Add 0.30 g of tetramethylammonium hydroxide dropwise and stir at 55° C. until no more gas is generated;
[0118] (6) Add 4.5 g of acidic cation exchange resin (NKC-9) and stir for 12 h; filter and distill the product to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)), the structural formula of which is:
[0119]
[0120] (7) Pour 16.2 g of boron nitride powder into 100 mL of nitric acid and stir at 60 °C for 12 h to obtain a pretreated dispersion;
[0121] (8) The pretreated dispersion was poured into a mixed solution of formic acid and sulfuric acid (volume ratio of 60:40) and stirred at 25° C. for 6 h to obtain a dispersion, which was then washed with water for multiple times and filtered until the pH value of the filtrate was 7.0 and then dried;
[0122] (9) adding the product of step (8) into DMF solvent to prepare a 35 mg / mL high dispersion, adding an aqueous solution of KH550 and stirring for 24 h, ultrasonically treating for 12 h and then centrifuging to obtain a modified hexagonal boron nitride nanosheet with a thickness of 2 nm in the supernatant;
[0123] (10) Add 30 g of P(OMS-ANI) into a stirring container, then add 10.5 g of thermally conductive filler-modified hexagonal boron nitride nanosheets, stir in a blender for 120 s, and then stir under vacuum for 60 s;
[0124] (11) Place the mixture in cold water and cool to room temperature, add 0.9 g of isopropyl titanate, stir for 120 s under vacuum, and then place the mixture in ice water and cool;
[0125] (12) Pour the cooled slurry onto a release film, form it into sheets using a roller press, and after curing, obtain an organic silicon self-healing thermal interface material with a thermal conductive filler mass fraction of 25%.
[0126] Comparative Example 1
[0127] Compared with Example 1, the only difference is that the boron nitride nanosheets are not modified. The specific steps are:
[0128] (1) Mix 1.5 g of octadecyl ammonium polyoxyethylene ether (PEGO) and 2.5 g of aniline (ANI) at 0°C and stir until uniform;
[0129] (2) adding 2.3 g of ammonium persulfate, carrying out polymerization reaction at 0° C. for 12 h, and then pouring out the product;
[0130] (3) The product was filtered and washed with pure water for 4 times to obtain polyaniline polymer (PANI);
[0131] (4) Add 8.5 g of PANI to 250 mL of hydrogenated silicone oil, add 300 mL of methanol solution, heat to 50 °C and stir evenly;
[0132] (5) Add 0.15 g of tetramethylammonium hydroxide dropwise and stir at 50° C. until no more gas is generated;
[0133] (6) Add 2.5 g of acidic cation exchange resin (NKC-9) and stir for 2 h; filter and distill the product to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)).
[0134] (7) Pour 10 g of boron nitride powder into 250 mL of nitric acid and stir at 50 °C for 12 h to obtain a pretreated dispersion;
[0135] (8) pouring the pretreated dispersion into a mixed solution of formic acid and sulfuric acid (volume ratio of 40:60) and stirring at 10° C. for 8 h to obtain a dispersion, washing with water for multiple times, neutralizing and filtering until the pH value of the filtrate is 5.5, and then drying to obtain unmodified hexagonal boron nitride nanosheets;
[0136] (9) Add 30 g of P(OMS-ANI) into a stirring container, then add 29.1 g of thermal conductive filler hexagonal boron nitride nanosheets, stir in a blender for 120 s, and then stir under vacuum for 60 s;
[0137] (10) Place the mixture in cold water and cool to room temperature, then add 0.9 g of isopropyl titanate, stir for 120 s under vacuum, and place the mixture in ice water to cool after stirring;
[0138] (11) Pour the cooled slurry onto a release film, form it into sheets through a roller press, and after curing, obtain a self-repairing thermal interface material with a thermal conductive filler mass fraction of 49%.
[0139] Comparative Example 2
[0140] Compared with Example 1, the only difference is that the organosilicon is not modified by polyaniline. The specific steps are:
[0141] (1) Add 300 mL of methanol solution to 250 mL of hydrogenated silicone oil and heat to 50 °C and stir evenly;
[0142] (2) adding 0.15 g of tetramethylammonium hydroxide dropwise and stirring at 50° C. until no more gas is generated;
[0143] (3) Add 2.5 g of acidic cation exchange resin (NKC-9) and stir for 2 h; filter and distill the product to obtain an organosilicon-polyaniline copolymer (P(OMS-ANI)).
[0144] (4) Pour 10 g of boron nitride powder into 250 mL of nitric acid and stir at 50 °C for 12 h to obtain a pretreated dispersion;
[0145] (5) pouring the pretreated dispersion into a mixed solution of formic acid and sulfuric acid (volume ratio of 40:60) and stirring at 10° C. for 8 h to obtain a dispersion, washing with water for multiple times and filtering until the pH value of the filtrate is 5.5, and then drying;
[0146] (6) adding the product of step (5) into DMF solvent to prepare a 25 mg / mL high dispersion, adding an aqueous solution of KH550 and stirring for 12 h, ultrasonically treating for 10 h and then centrifuging to obtain modified hexagonal boron nitride nanosheets with a thickness of 3 nm in the supernatant;
[0147] (7) Add 30 g of P(OMS-ANI) into a stirring container, then add 29.1 g of thermal conductive filler hexagonal boron nitride nanosheets, stir in a blender for 120 s, and then stir under vacuum for 60 s;
[0148] (8) Place the mixture in cold water and cool to room temperature, then add 0.9 g of isopropyl titanate, stir for 120 s under vacuum, and place the mixture in ice water to cool after stirring;
[0149] (9) Pour the cooled slurry onto a release film, form a sheet through a roller press, and solidify to obtain a self-repairing thermal interface material with a thermal conductive filler mass fraction of 45%.
[0150] Comparative Example 3
[0151] Compared with Example 1, the only difference is that the organosilicon is a product of cross-linking hydrogenated silicone oil with vinyl silicone oil through a hydrosilylation reaction, and the specific steps are:
[0152] (1) Add 300 mL of methanol solution to 250 mL of hydrogenated silicone oil and heat to 50 °C and stir evenly;
[0153] (2) adding 0.15 g of tetramethylammonium hydroxide dropwise and stirring at 50° C. until no more gas is generated;
[0154] (3) adding 2.5 g of acidic cation exchange resin (NKC-9) and stirring for 2 h; filtering and distilling the product to obtain a hydrogenated silicone oil pretreatment liquid.
[0155] (4) Pour 10 g of boron nitride powder into 250 mL of nitric acid and stir at 50 °C for 12 h to obtain a pretreated dispersion;
[0156] (5) pouring the pretreated dispersion into a mixed solution of formic acid and sulfuric acid (volume ratio of 40:60) and stirring at 10° C. for 8 h to obtain a dispersion, washing with water for multiple times and filtering until the pH value of the filtrate is 5.5, and then drying;
[0157] (6) adding the product of step (5) into DMF solvent to prepare a 25 mg / mL high dispersion, adding an aqueous solution of KH550 and stirring for 12 h, ultrasonically treating for 10 h and then centrifuging to obtain modified hexagonal boron nitride nanosheets with a thickness of 3 nm in the supernatant;
[0158] (7) Add 30 g of hydrogenated silicone oil pretreatment liquid into a stirring container, then add 29.1 g of thermal conductive filler hexagonal boron nitride nanosheets, stir in a stirrer for 120 s, and then stir under vacuum for 60 s;
[0159] (8) Place in cold water and cool to room temperature, add 3.7 g of vinyl silicone oil (Runhe, RH-Vi395), then add 0.9 g of isopropyl titanate, stir under vacuum for 120 s, and place in ice water to cool after stirring;
[0160] (9) Pour the cooled slurry onto a release film, form it into sheets through a roller press, and obtain a self-repairing thermal interface material with a thermal conductive filler mass fraction of 46% after solidification.
[0161] The organic silicon self-repairing thermal interface materials obtained from the above-mentioned examples and comparative examples were subjected to thermal conductivity tests and self-repairing performance tests.
[0162] Thermal conductivity test
[0163] Samples with a diameter of 3 cm and thicknesses of 1 mm, 2 mm and 3 mm were prepared, and the thermal conductivity of the samples was measured using a thermal conductivity tester. The results are shown in Table 1.
[0164] Table 1
[0165]
[0166]
[0167] The thermal conductivity of the product of Example 1 is 9.324W / mK. The samples of Example 1 with three thicknesses were cut with a knife, and the thermal conductivity was measured and calculated after self-repairing for 2-6 hours. The data is the data after self-repairing once; the samples of three thicknesses were cut with a knife again, and the thermal conductivity was measured and calculated after self-repairing for a period of time. The results are as follows Figure 5As shown, the thermal conductivity of Example 1 after self-repairing once and twice is 9.304 W / mK, indicating that the thermal conductivity of the organic silicon self-repairing thermal interface material remains unchanged after self-repairing.
[0168] Tensile properties test
[0169] The product of Example 1 was prepared into a bone-shaped sample, and its tensile properties were tested using a universal testing machine at a speed of 10 mm / min. The product of Example 1 was prepared into a bone-shaped sample, cut in the middle with a knife, and the cuts were put together. After self-repairing for a period of time at room temperature, its tensile properties were tested using a universal testing machine at a speed of 10 mm / min. The tensile curves before and after self-repair are shown in Figure 1. Figure 2 As shown in the figure, it can be seen that the elongation does not change significantly after self-repairing.
[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An organosilicon-polyaniline copolymer, characterized in that: The structural formula of the organosilicon-polyaniline copolymer is: Among them, POMS is pendant alkoxy polysiloxane, and PANI is polyaniline; Among them, R1, R2, R3, R4, R7, and R8 are independently selected from one of methyl, ethyl, or propyl, and R5 and R6 are independently selected from one of methyl, ethyl, trifluoropropyl, or phenyl; m and o are independently natural numbers of 20 to 5000, and n and p are independently natural numbers of 50 to 1500.
2. The organosilicon-polyaniline copolymer according to claim 1, characterized in that: The m, n, o, and p satisfy: (n+p) / (m+n+o+p)*100%=5-45%, preferably 15-36%.
3. The organosilicon-polyaniline copolymer according to claim 1, characterized in that: y and z are respectively and independently natural numbers ranging from 100 to 1500, and the value of y / (y+z) is 25 to 85%, preferably 35 to 65%.
4. A method for preparing the organosilicon-polyaniline copolymer according to any one of claims 1 to 3, characterized in that: The following steps are involved: (a) adding polyaniline to hydrogen-containing silicone oil, and then adding an organic solvent to mix well; (b) adding tetramethylammonium hydroxide to the uniformly mixed solution, and stirring the reaction until no gas is generated; (c) adding an acidic cation exchange resin, stirring and then filtering to obtain the organosilicon-polyaniline copolymer.
5. The preparation method according to claim 4, characterized in that: The organic solvent in step (a) is selected from methanol; Preferably, the stirring reaction temperature in step (b) is 30 to 80° C.; Preferably, in the step (a), the usage ratio of polyaniline to hydrogen-containing silicone oil is (5.6-13.5) g: (200-450) mL.
6. A silicone-polyaniline copolymer self-repairing thermal interface material, characterized in that: The raw materials of the self-repairing thermal interface material include: organic silicon-polyaniline copolymer, isopropyl titanate and thermal conductive filler, wherein the organic silicon-polyaniline copolymer is as described in any one of claims 1 to 3 or is obtained by the preparation method of claim 4 or 5.
7. The organosilicon-polyaniline copolymer self-repairing thermal interface material according to claim 6, characterized in that: The thermal conductive filler is a modified hexagonal boron nitride nanosheet; Preferably, the mass fraction of the thermal conductive filler in the raw material is 35-75%, preferably 45-65%; Preferably, in the mixture of the organosilicon-polyaniline copolymer and isopropyl titanate, the mass fraction of the organosilicon-polyaniline copolymer is 95-98%, and the mass fraction of the isopropyl titanate is 2-5%.
8. The organosilicon-polyaniline copolymer self-repairing thermal interface material according to claim 6, characterized in that: The preparation process of the modified hexagonal boron nitride nanosheets comprises: S1. Mixing boron nitride powder and nitric acid and stirring at 10-70° C. for 4-24 hours to obtain a pre-treated dispersion; S2, adding the pretreated dispersion into a mixed solution of formic acid and sulfuric acid, stirring at 0-50°C for 1-12h to obtain a dispersion, washing with water for multiple times, neutralizing and filtering until the pH value of the filtrate is 5.0-7.5, and then drying; S3, adding the product into a solvent to prepare a highly dispersed liquid, adding a silane coupling agent and stirring for 4 to 24 hours, ultrasonically treating for 8 to 24 hours and then centrifuging to obtain the modified hexagonal boron nitride nanosheets with a thickness of 1 to 4 nm in the supernatant.
9. A method for preparing the organosilicon-polyaniline copolymer self-repairing thermal interface material according to any one of claims 6 to 8, characterized in that: The following steps are involved: (1) mixing the organosilicon-polyaniline copolymer and the thermal conductive filler, stirring under vacuum conditions, and cooling to room temperature; (2) adding isopropyl titanate, stirring under vacuum conditions, and cooling after stirring; (3) pouring the cooled slurry onto a release film, forming a sheet through a roller press, and obtaining the organosilicon-polyaniline copolymer self-healing thermal interface material after curing.
10. The preparation method according to claim 9, characterized in that: The cooling in step (2) refers to cooling with ice water at 0 to 8°C; Preferably, the stirring time under vacuum conditions in step (1) and step (2) is 30 to 180 seconds.
Citation Information
Patent Citations
Low-emission high-performance heat-conducting silicone grease and preparation method thereof
CN118027674A