Preparation method and application of triphenylene long-afterglow elastic film
By mixing tribenzene with flexible polymer SEBS, a tribenzene long afterglow elastic film with long afterglow time and good tensile properties is formed, which solves the problems of short afterglow time, poor luminescence uniformity and poor tensile properties of the material in the prior art. , realizes efficient organic long afterglow materials suitable for flexible display and anti-counterfeiting.
Patent Information
- Application Number
- CN202411205022.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing preparation methods for organic long afterglow materials, the material has a short afterglow time, poor luminescence uniformity, and poor tensile performance, making it difficult to meet the needs of flexible display technology, wearable devices and high-end anti-counterfeiting fields.
By mixing triphenylene with flexible polymer SEBS, a triphenylene long afterglow elastic film is formed, the rigid environment is constructed using the denseness of SEBS, non-radiative transitions are suppressed, and large-area coating and stretchability are achieved through its elasticity, thereby improving afterglow Time and luminous uniformity.
The prepared tribylene long afterglow elastic film has an afterglow time of up to 8 seconds, good tensile performance and luminous uniformity. It is suitable for flexible display, anti-counterfeiting and biological detection. The material is simple, cheap and does not require high temperature and high pressure conditions.
Smart Images

Figure CN118930922A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of organic long afterglow material preparation methods, in particular to a preparation method and application of a triphenylene long afterglow elastic film. Background Art
[0002] Organic long-persistent luminescence (OLPL) materials have advantages such as easy synthesis, functional modification and processing, and the ability to control persistent room-temperature phosphorescence (PRTP) through reasonable molecular design. They show potential application prospects in bioimaging, photodynamic therapy, information storage anti-counterfeiting, sensing, electroluminescent devices and security protection. In the field of OLPL research, no matter how the research system changes, how to improve the PRTP efficiency (luminescence brightness and duration) is the top priority for researchers. At present, the methods to improve OLPL mainly focus on two aspects: 1) The intersystem crossing efficiency can be significantly improved by modifying heteroatom and carbonyl functional groups, or by using heavy atom effects or polymers to enhance intersystem crossing, thereby enhancing spin-orbit coupling, thereby generating long-lived triplet states to induce observable PRTP phenomena; 2) Long-lived triplet states are very sensitive to oxygen and molecular vibrations, and the construction of crystals, MOFs, H aggregation and other systems can use the rigid environment of the system to reduce the non-radiative transition of triplet states and further improve the efficiency of PRTP emission; however, while constructing a rigid environment, the flexibility of the material will inevitably be weakened, which is a bottleneck problem for large-area and flexible applications of the material. Therefore, the development of afterglow materials with high-efficiency luminescence and excellent stretchability for application in flexible display technology, wearable devices, high-end anti-counterfeiting and biological detection fields is a problem that needs to be solved urgently.
[0003] In our previous research, we have solved this problem by adding high molecular polymers to prepare flexible films. By adding condensed ring compounds benzophenone and tetracene to the flexible polymer SEBS, we prepared an elastic polymer film with long afterglow performance, which changed the elasticity and flexibility of the material. However, the afterglow time of the prepared elastic film is short, and more importantly, the luminous uniformity is poor. How to develop more materials to achieve dynamic control of afterglow time is currently the top priority in this field. Summary of the invention
[0004] The invention provides a preparation method and application of a triphenylene long afterglow elastic film, so as to solve the problems of short afterglow time, poor luminous uniformity and poor tensile performance of an OLPL film prepared by a prior art OLPL material preparation method.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is: The preparation method of triphenylene long afterglow elastic film comprises the following steps: adding triphenylene and styrene-ethylene-butylene-styrene as solutes into a solvent, and stirring the solvent at a temperature of 60°C to 80°C to allow the solutes to be completely dispersed and dissolved in the solvent, thereby forming a mixed solution; then, drop-coating the mixed solution onto a substrate to form a film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining the triphenylene long afterglow elastic film.
[0006] Among them, the structural formula of triphenylene is:
[0007] The structural formula of styrene-ethylene-butylene-styrene is:
[0008] Furthermore, in the solute, the mass ratio of triphenylene to styrene-ethylene-butylene-styrene is 1:200.
[0009] Furthermore, the solvent is toluene.
[0010] Furthermore, the total mass of the solute added per 1 ml of toluene is 201 mg to 402 mg.
[0011] The triphenylene long afterglow elastic film prepared by the method for preparing the triphenylene long afterglow elastic film is used as a flexible afterglow material in electronic devices.
[0012] The invention discloses an application of the triphenylene long afterglow elastic film prepared by the method for preparing the triphenylene long afterglow elastic film as an anti-counterfeiting mark.
[0013] The triphenylene long afterglow elastic film prepared by the method for preparing the triphenylene long afterglow elastic film is used as a marker in biological detection.
[0014] In the present invention, from the perspective of improving the large-area coating and stretchability of organic long afterglow film materials, triphenylene is incorporated into the flexible polymer styrene ethylene butylene styrene (SEBS), and triphenylene is used as a luminescent body, which has a simple structure and is easy to obtain. The compactness of the flexible polymer SEBS is used to construct a rigid environment to inhibit non-radiative transitions. More importantly, the flexible polymer SEBS has the ability to separate oxygen, greatly improving the room temperature phosphorescence of organic molecules and obtaining an afterglow time of up to 8 s; at the same time, the elasticity of the flexible polymer SEBS is used to achieve large-area coating and stretchability of the material, and uniform luminescence, which provides a good basis for preparing triphenylene long afterglow elastic film.
[0015] The triphenylene long afterglow elastic film prepared by the preparation method of the triphenylene long afterglow elastic film provided by the present invention has good afterglow luminescence performance, can form a uniform, transparent, flexible and stretchable large-area film, and its stretching performance is the best among polymer long afterglow materials, can be repeatedly stretched for many times, and has the advantages of long afterglow time and uniform luminescence. The preparation method of the present invention is simple, the material is cheap and easy to obtain, the conditions are mild and harsh conditions such as high temperature and high pressure are not required, which is very beneficial to the application of organic LPL materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 This is the tensile stress-strain curve of TP@SEBS obtained in Example 1.
[0017] Figure 2 These are optical micrographs of the TP@SEBS obtained in Example 1 before and after illumination and an optical photograph showing afterglow.
[0018] Figure 3 This is the afterglow time decay curve of TP@SEBS obtained in Example 1.
[0019] Figure 4 This is the RTP performance of triphenylene (TP) and SEBS blend (TP@SEBS) under strain in Example 1 (photo).
[0020] Figure 5 These are RTP photographs of the TP@SEBS elastic film obtained in Example 1 under bending, rolling and torsion conditions.
[0021] Figure 6 The TP@SEBS elastic film obtained in Example 1 has a SEBS film with a “√” pattern and plays an anti-counterfeiting role in the handle of a badminton racket.
[0022] Figure 7 Optical micrographs of BP@SEBS obtained in the comparative example before and after illumination and an optical photograph showing afterglow. DETAILED DESCRIPTION
[0023] The present invention is further described below in conjunction with the accompanying drawings and embodiments. Example
[0024] A preparation method of a triphenylene long afterglow elastic film TP@SEBS, the process is as follows: Triphenylene (TP) and the flexible polymer styrene ethylenebutylene styrene (SEBS) were used as solutes and toluene was used as solvent. Due to the good solubility of SEBS and TP in toluene, they can be mixed well.
[0025] Among them, the purchaser of triphenylene is Beijing Inokai Technology Co., Ltd. (purity: 97%), and the structural formula of triphenylene is:
[0026] The structural formula of styrene-ethylene-butylene-styrene is:
[0027] In the solute, the mass ratio of triphenylene to styrene-ethylene-butylene-styrene is 1:200, and the total mass of the solute added per 1 ml of toluene is 201 mg~402 mg.
[0028] In this embodiment, 2 mg of triphenylene, 400 mg of styrene-ethylene-butylene-styrene, and 1 ml of toluene are taken. 2 mg of triphenylene and 400 mg of styrene-ethylene-butylene-styrene are added to 1 ml of toluene, and stirred at a temperature of 60° C. to 80° C. to make the triphenylene and styrene-ethylene-butylene-styrene completely and evenly dispersed and dissolved in toluene, thereby forming a mixed solution.
[0029] Then, a glass substrate is used as a substrate, and the mixed solution is drop-coated on the glass substrate to form a thin film. After the thin film is naturally cooled at room temperature of 20-25°C, the thin film on the glass substrate is transferred to a mold, and the solvent is naturally evaporated in the mold at room temperature of 20-25°C. The residue obtained is the triphenylene long afterglow elastic film TP@SEBS. In the obtained triphenylene long afterglow elastic film TP@SEBS, TP is uniformly dispersed in SEBS, and the obtained triphenylene long afterglow elastic film TP@SEBS has the advantages of good stretchability, long afterglow time, and uniform luminescence.
[0030] The following describes the performance of the triphenylene long afterglow elastic film TP@SEBS prepared in this embodiment in combination with the images obtained in the experiment. During the experiment, the optical performance measurement instrument uses an Ocean Optics multi-band spectrometer, and the mechanical performance measurement instrument uses an electronic universal tensile testing machine MTS CMT4000.
[0031] Figure 1 is the tensile stress-strain curve of the triphenylene long afterglow elastic film TP@SEBS obtained in this example, Figure 1 It can be seen that at a constant strain rate of 2 mm·s −1 Under the conditions of , the long afterglow material with RTP performance showed excellent stretchability and was able to be stretched to about 420% of its original length. The tensile properties of the blended material were very similar to those of pure SEBS (about 445% of its original length), indicating that even trace amounts of phosphors do not affect the tensile properties of SEBS.
[0032] Figure 2 This is the macroscopic LPL picture of the triphenylene long afterglow elastic film TP@SEBS obtained in this example at room temperature. It can be seen that the obtained polymer film emits light more uniformly. Figure 2 It can be seen that when the film is excited by 365 nm ultraviolet light, the fluorescence color emitted by the film is blue. After irradiation for 3 seconds, the excitation light source is turned off and the polymer film can emit green afterglow (such as Figure 2 a), in the first 3 s ( Figure 2 b represents the first s, Figure 2 c represents the 2nd s, Figure 2 d represents the 3rd s) the afterglow brightness of the compound is stronger, from the 4th s (such as Figure 2 e) and then the afterglow gradually weakened. At 5 s ( Figure 1 f) 6th s ( Figure 2 g) and 7 s ( Figure 2 h) and the afterglow further weakened. At 8 s ( Figure 2 i) Afterglow is about to disappear. The above results show that the afterglow time of the triphenylene long afterglow elastic film TP@SEBS reaches about 8 s, with good afterglow performance, and the whole film emits light uniformly. This is mainly attributed to the rigid environment formed by the SEBS polymer and its ability to effectively isolate oxygen. The introduction of the SEBS polymer can effectively trigger the luminescence performance of the guest material.
[0033] The afterglow performance attenuation of the triphenylene long afterglow elastic film TP@SEBS obtained in this embodiment was tested using an Ocean Optics multi-band spectrometer. The results are as follows: Figure 3 shown. Figure 3 In the figure, -2 s to 0 s is the triphenylene long afterglow elastic film TP@SEBS under 365nm ultraviolet light, which shows photoluminescence characteristics; 0 s to 10 s is the triphenylene long afterglow elastic film TP@SEBS after the ultraviolet light is removed, which shows green long afterglow light, and the afterglow time is about 8 s, which is similar to the afterglow time observed by the naked eye.
[0034] In order to better verify the luminescence performance and stretchability of this type of material, this example conducted a luminescence test on the triphenylene long afterglow elastic film TP@SEBS when stretched. Figure 4 As shown in the figure, the blend of triphenylene (TP) and polymer SEBS (TP@SEBS) can induce afterglow luminescence for more than 8 s. By stretching the elastomer film test, the long-lasting afterglow performance can be clearly observed even in the deformation area. The photophysical properties of TP@SEBS under different stretching states (0~100%) show that the RTP strength of the blend material drops to 85% of the original, indicating that the blend material has good anti-deformation performance.
[0035] Taking advantage of the excellent stretchability and ambient multicolor afterglow of this type of hybrid materials, this example further studies their potential applications in flexible display, dynamic information encryption, anti-counterfeiting, and oxygen detection.
[0036] Initially, the triphenylene long-lasting elastic film TP@SEBS was transformed into long and thin lines that could be easily stretched under tension to demonstrate the material’s stretchability. Figure 5 As shown, these lines can be effortlessly molded into various shapes while maintaining durable RTP even after rolling, suggesting that they can easily create a variety of flexible patterns for decorative purposes.
[0037] like Figure 6 As shown in Figure 2, SEBS has the potential to be used in the production of handles for sports equipment, such as badminton rackets and table tennis rackets, due to its good wear resistance and water resistance. In addition, the addition of phosphors enables SEBS materials to effectively present various patterns of different shapes, and ultraviolet light sources can conveniently verify the patterns displayed on SEBS, thereby realizing the preparation of anti-counterfeiting labels.
[0038] Therefore, the triphenylene long afterglow elastic film TP@SEBS prepared in this embodiment can be used as a flexible afterglow material in flexible display electronic devices, wearable electronic devices, and portable electronic devices, and can also be used as an anti-counterfeiting marker and as a marker in biological detection.
[0039] Comparative Example The comparative example provides a method for preparing an organic-doped elastic film that can be coated over a large area and has a stretching function, comprising the following steps: The condensed ring compound phenylene (BP) (5 mol‰, 2 mg) and the polymer styrene ethylene butylene styrene (SEBS) (400 mg) were added to toluene (1 ml) and dissolved by stirring at 60℃~80℃. Due to the good solubility of SEBS and condensed ring polymer BP in toluene, they can be mixed well, and the well-dispersed mixed solution is dropped on a glass substrate. After natural cooling, the mixture is transferred to a mold, and the elastomeric polymer film is obtained after the solvent evaporates.
[0040] The structural formula of the condensed ring compound triphenylene BP is:
[0041] The structural formula of SEBS is: Figure 7This is a macroscopic LPL picture of the elastomeric polymer film obtained in the comparative example at room temperature. It can be seen that the obtained polymer film emits light more evenly. Figure 7 It can be seen that when the film is excited by 365 nm ultraviolet light, the fluorescence color emitted by the film is blue. After irradiation for 3 seconds, the excitation light source is turned off and the polymer film can emit green afterglow (such as Figure 7 a), in the first 3 s ( Figure 7 b represents the first s, Figure 7 c represents the 2nd s, Figure 5 d represents the 2nd s) the afterglow brightness of the compound is stronger, from the 4th s (such as Figure 7 e) and then the afterglow gradually weakened, reaching the 5th second (as shown in Figure 7 f) has a weak afterglow, and the 6th s (as shown in Figure 7 The above results show that the afterglow time of the polymer film prepared in the comparative example reaches about 5 s. Although it has good afterglow performance, the luminous uniformity of the entire film is poorer than that of the triphenylene long afterglow elastic film TP@SEBS prepared in Example 1.
[0042] The preferred embodiments of the present invention are described in detail above in conjunction with the accompanying drawings. The embodiments described in the present invention are merely descriptions of the preferred embodiments of the present invention, and do not limit the concept and scope of the present invention. The various specific technical features described in the above specific embodiments can be combined in any suitable manner without contradiction, and such combinations should also be regarded as the contents disclosed in the present disclosure as long as they do not violate the concept of the present invention. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.
[0043] The present invention is not limited to the specific details of the above-mentioned embodiments. Within the technical concept of the present invention and without departing from the design concept of the present invention, various modifications and improvements made to the technical solution of the present invention by technical personnel in this field should fall within the protection scope of the present invention. The technical contents for which protection is sought in the present invention have been fully recorded in the claims.
Claims
1. A method for preparing a triphenylene long afterglow elastic film, characterized in that: Triphenylene and styrene-ethylene-butylene-styrene are added as solutes into a solvent, and stirred at a temperature of 60°C to 80°C to allow the solutes to be completely dispersed and dissolved in the solvent, thereby forming a mixed solution; then, the mixed solution is drop-coated onto a substrate to form a thin film, and after the film is naturally cooled at room temperature, the solvent is naturally evaporated at room temperature, thereby obtaining a triphenylene long afterglow elastic film.
2. The method for preparing the triphenylene long afterglow elastic film according to claim 1, characterized in that: In the solute, the mass ratio of triphenylene to styrene-ethylene-butylene-styrene is 1:
200.
3. The method for preparing the triphenylene long afterglow elastic film according to claim 2, characterized in that: The solvent is toluene.
4. The method for preparing the triphenylene long afterglow elastic film according to claim 3, characterized in that: The total mass of solute added per 1 ml of toluene is 201 mg~402 mg.
5. Use of the triphenylene long afterglow elastic film prepared by the method for preparing the triphenylene long afterglow elastic film as claimed in any one of claims 1 to 4 as a flexible afterglow material in electronic devices.
6. Use of a triphenylene long afterglow elastic film prepared by the method for preparing a triphenylene long afterglow elastic film as claimed in any one of claims 1 to 4 as an anti-counterfeiting marker.
7. Use of the triphenylene long afterglow elastic film prepared by the method for preparing the triphenylene long afterglow elastic film as claimed in any one of claims 1 to 4 as a marker in biological detection.