Preparation method of modified PVC (polyvinyl chloride) heat-shrinkable label film
By adding PETG and modified silica to the PVC resin, the problem of insufficient shrinkage and cold resistance of the polyvinyl chloride heat shrink film is solved, and a modified PVC heat shrinkage label film with high shrinkage and cold resistance is achieved. It is suitable for Packaging and low temperature environment with large size variations.
Patent Information
- Application Number
- CN202411221951.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The maximum shrinkage rate of polyvinyl chloride heat shrink film is generally around 50%, which cannot meet the packaging requirements of large size variations and is not suitable for low-temperature environments.
PETG is used to improve the heat shrinkage rate of PVC resin, and improve the heat shrinkage rate and cold resistance by modifying silica as a toughening agent. The specific method includes adding PETG and modified silica to the PVC resin, using ionic liquid as melt compatibility promoter, and modifying silica forms a porous structure through ultrasonic dispersion and spray deposition, combining with methyl short branched structure, Improve the toughness and thermal stability of the material.
The maximum shrinkage rate of heat shrink film is achieved to reach 80%, and significantly improves cold resistance and thermal stability, suitable for a wider range of packaging needs and low temperature environments.
Smart Images

Figure BDA0005023291790000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat shrinkable label films, and in particular relates to a preparation method of a modified PVC heat shrinkable label film. Background Art
[0002] PVC heat shrink film is made by mixing ethylene-based PVC with auxiliary materials and then inflating it twice. It is widely used in the packaging of various commodities such as wine, food, sports goods, sterilized tableware, electronic appliances, daily necessities, handicrafts, health products, audio-visual products, medicines, stationery, toys, doors, plastic hardware, glass and ceramics, etc., making the appearance more vivid and beautiful, improving the grade of product packaging, and protecting the product from dust and waste. It is an ideal film packaging material. PVC heat shrink label film is affected by the molecular structure of its own material. The maximum shrinkage rate of the label film is generally around 50%, and the maximum does not exceed 60%. It cannot meet the packaging requirements with large dimensional changes, and is not suitable for low temperature environments. Summary of the invention
[0003] In view of the problems in the prior art, the present invention provides a method for preparing a modified PVC heat shrinkable label film, which solves the defects of PVC, utilizes PETG to improve the heat shrinkage rate of PVC resin, and uses modified silica as a toughening agent to improve the cold resistance of PVC material on the basis of increasing the heat shrinkage rate.
[0004] In order to achieve the above technical objectives, the technical solution of the present invention is:
[0005] A method for preparing a modified PVC heat shrinkable label film, wherein the mass ratio of the label film is:
[0006] 100 parts of PVC resin, 15-25 parts of PETG, 0.18-0.45 parts of plasticizer, 2-5 parts of toughening agent, 3-5 parts of processing aid, 0.5-0.7 parts of lubricant, and 0.2-0.4 parts of stabilizer.
[0007] The PETG is also known as polyethylene terephthalate-1,4-cyclohexane dimethanol, which is a transparent, non-crystalline copolyester; the heat shrink film prepared from this material has a high shrinkage rate, the maximum shrinkage rate can reach 80%, and has good cold resistance. Adding PETG to PVC resin can effectively improve the cold resistance of PVC and can also correspondingly improve the shrinkage rate of PVC heat shrink label film.
[0008] The plasticizer is an ionic liquid, specifically 1-ethyl phosphate-3-methylimidazolium chloride. There are certain differences in melting point and rheology between PVC resin and PETG, resulting in uneven mixing during melt blending and extrusion film blowing. The ionic liquid, as a melt compatibility promoter for the two materials, plasticizes PETG and affects the rheological properties of the PETG melt, ensuring that the rheological properties of PETG and PVC are consistent and improving the consistency of the melt flow of the two materials. The negative ion Cl in the ionic liquid - The structure of chlorine is the same as that of PVC molecular structure, which can enhance the interfacial bonding force between PVC and PETG and achieve better miscibility.
[0009] The toughening agent uses modified silica, which has high surface energy and small particle size, and can effectively improve the toughness and flame retardancy of the material. However, silica itself has a certain inertness. The inert silica has little effect in the initial stage of the label film. As the material on the label film ages, the inertness problem of the silica surface becomes prominent, causing the label film to become powdery. To address this problem, the toughening agent uses long-chain modified silica in a mesoporous system. The mesoporous structure can increase the specific surface area, protect the label film, improve the elastic modulus and wear resistance, and improve thermal stability. Qualitative; The preparation method of the modified silicon dioxide comprises the following steps: a1, adding trichlorophenylsilane, ethyl cellulose and ethyl silicate to ether and stirring evenly to form a mixed solution, spraying it into a reaction kettle for deposition to form particles after ultrasonic dispersion, and obtaining porous silicon dioxide particles after soaking and drying, wherein the molar ratio of the trichlorophenylsilane, ethyl cellulose and ethyl silicate is 2-3:1-2:2, the concentration of the trichlorophenylsilane in ether is 300-400g / L, the stirring speed for uniform stirring is 300-500r / min, and the ultrasonic frequency of the ultrasonic dispersion is 80- 100kHz, temperature is 10-20℃; the spray speed is 5-8mL / min, the spray atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 8-10:1, and the deposition temperature is 60-70℃; the solvent for soaking and drying is ethanol, and the drying temperature is 90-100℃; this step utilizes trichlorophenylsilane, ethyl cellulose and ethyl silicate all have good solubility in ether, and form a homogeneous dispersion in ultrasonic treatment, and is removed by hydrolysis and polycondensation in the spray deposition process and ethyl cellulose in soaking and drying, thereby forming a2, soaking the porous silica particles in an acid solution for 1-2 hours, filtering and drying to obtain acidified silica particles, wherein the concentration of the porous silica particles in the acid solution is 100-400 g / L, the acid solution is a hydrochloric acid solution with a pH of 5-6, the soaking temperature is 20-30° C., and the drying temperature is 100-120° C. This step uses the soaking and acid washing method to activate the surface of the porous silica particles, thereby providing conditions for the subsequent coupling reaction;a3, dimethyldimethoxysilane is placed in ether to form a dilute solution, and then acidified silica is placed and a small amount of distilled water is added, and the solution is filtered after ultrasonic treatment, and the solution is dried by spraying powder to obtain modified porous silica particles, wherein the concentration of the dimethyldimethoxysilane in ether is 10-40 g / L, the concentration of the acidified silica in ether is 100-300 g / L, the amount of distilled water added is 120-150% of the molar amount of the dimethyldimethoxysilane, the ultrasonic frequency of the ultrasonic treatment is 80-100 kHz, the temperature is 5-10° C., and the atmosphere of the spraying powder drying is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 8 -10:1, the temperature is 90-100°C; this step utilizes the solubility of ether in dimethyldimethoxysilane to homogeneously disperse dimethyldimethoxysilane, and cooperates with the homogeneous dispersion of acid-activated porous silica particles and the penetration and hydrolysis of distilled water to disperse and fix dimethyldihydroxysilane after the hydrolysis of dimethyldimethoxysilane on the porous silica particles. The modified porous silica particles use dimethylsilane as a branched structure and porous silica as a framework. The porous structure interacts with the resin structure during operations such as melt extrusion, and cooperates with the methyl short branch structure to achieve structural stability under the physical system; the surface is rich in silanol and phenyl groups, which improves thermal stability and wear resistance. ;
[0010] The processing aid is ACR processing aid, which can improve the processing rheology of PVC, promote plasticization and improve melt ductility.
[0011] The lubricant is oxidized polyethylene wax, which is a polar wax with a unique molecular structure and a certain amount of carbonyl and hydroxyl groups. It not only plays an external lubrication and demolding role, reduces the adhesion of the melt, thereby improving the overall demolding property, but also plays an internal lubrication role, reduces the melt viscosity, improves the melt fluidity, and thus increases the processing production rate.
[0012] The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 3-4:1.
[0013] The preparation method of the modified PVC heat shrinkable label film comprises the following steps:
[0014] Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry mix, the stirring speed is 2000-3000r / min, and the temperature is 5-10°C;
[0015] Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 145-190° C.;
[0016] Step 3, after mixing PVC masterbatch, PETG and plasticizer, adding them into a single screw extruder for melt extrusion, and blowing them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 155-215° C., the water bath heating temperature before the two-bubble blowing is 85-89° C., and the two-bubble blowing ratio is 2.4-2.8; the PETG is ground before use.
[0017] It can be seen from the above description that the present invention has the following advantages:
[0018] 1. The present invention solves the defects of PVC, uses PETG to improve the heat shrinkage rate of PVC resin, and uses modified silicon dioxide as a toughening agent to improve the cold resistance of PVC materials on the basis of increasing the heat shrinkage rate.
[0019] 2. The present invention utilizes the silane coupling modification of modified silica itself and the methyl short-chain branch on silane, which not only improves the long-term stability of silica, but also reduces the surface inertness of silica particles through activity and modification.
[0020] 3. The present invention uses ionic liquid as a plasticizer, which can be used as a melt compatibility promoter for PVC and PETG, making the melt fluidity of PETG and PVC tend to be consistent, thereby achieving high-quality miscibility. DETAILED DESCRIPTION
[0021] The present invention is described in detail with reference to the embodiments, but no limitation is imposed on the claims of the present invention.
[0022] Example 1
[0023] A method for preparing a modified PVC heat shrinkable label film, wherein the mass ratio of the label film is:
[0024] 100 parts of PVC resin, 15 parts of PETG, 0.18 parts of plasticizer, 2 parts of toughening agent, 3 parts of processing aid, 0.5 parts of lubricant, and 0.2 parts of stabilizer.
[0025] The plasticizer is 1-ethyl phosphate-3-methyl imidazolium chloride.
[0026] The toughening agent adopts modified silica, and the modified silica uses dimethylsilane as a branched structure and porous silica as a framework; the preparation method of the modified silica comprises the following steps: a1, adding trichlorophenylsilane, ethyl cellulose and ethyl silicate into ether and stirring evenly to form a mixed solution, spraying into a reaction kettle for deposition to form particles after ultrasonic dispersion, and obtaining porous silica particles by soaking and drying, wherein the molar ratio of the trichlorophenylsilane, ethyl cellulose and ethyl silicate is 2:1:2, the concentration of the trichlorophenylsilane in ether is 300g / L, the stirring speed for uniform stirring is 300r / min, the ultrasonic frequency of the ultrasonic dispersion is 80kHz, and the temperature is 10°C; the spraying speed is 5mL / min, the spraying atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 8:1, and the deposition temperature is 60°C; the solvent for soaking and drying is ethanol, and the drying temperature is 90°C a2, soak the porous silica particles in an acid solution for 1 hour, filter and dry to obtain acidified silica particles, the concentration of the porous silica particles in the acid solution is 100 g / L, the acid solution uses a hydrochloric acid solution with a pH of 5, and the soaking temperature is 20°C; the drying temperature is 100°C; a3, put dimethyldimethoxysilane into ether to form a dilute solution, then put the acidified silica into it and add a small amount of distilled water, filter after ultrasonic treatment, and spray dry to obtain modified porous silica particles, the concentration of the dimethyldimethoxysilane in ether is 10 g / L, the concentration of the acidified silica in ether is 100 g / L, the amount of distilled water added is 120% of the molar amount of dimethyldimethoxysilane, the ultrasonic frequency of the ultrasonic treatment is 80 kHz, the temperature is 5°C, the atmosphere of the spray drying is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 8:1, and the temperature is 90°C.
[0027] The processing aid is ACR processing aid HF-401.
[0028] The lubricant is oxidized polyethylene wax.
[0029] The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 3:1.
[0030] The preparation method of the modified PVC heat shrinkable label film comprises the following steps:
[0031] Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry mix, the stirring speed is 2000r / min, and the temperature is 5°C;
[0032] Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 145° C.;
[0033] Step 3, after mixing PVC masterbatch, PETG and plasticizer, adding them into a single screw extruder for melt extrusion, and blowing them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 155° C., the water bath heating temperature before the two-bubble blowing is 85° C., and the two-bubble blowing ratio is 2.4; the PETG is ground before use.
[0034] Example 2
[0035] A method for preparing a modified PVC heat shrinkable label film, wherein the mass ratio of the label film is:
[0036] 100 parts of PVC resin, 25 parts of PETG, 0.45 parts of plasticizer, 5 parts of toughening agent, 5 parts of processing aid, 0.7 parts of lubricant, and 0.4 parts of stabilizer.
[0037] The plasticizer is 1-ethyl phosphate-3-methyl imidazolium chloride.
[0038] The toughening agent adopts modified silica, and the modified silica uses dimethylsilane as a branched structure and porous silica as a framework; the preparation method of the modified silica comprises the following steps: a1, adding trichlorophenylsilane, ethyl cellulose and ethyl silicate into ether and stirring evenly to form a mixed solution, spraying the mixed solution into a reactor for deposition to form particles after ultrasonic dispersion, and obtaining porous silica particles by soaking and drying, wherein the molar ratio of the trichlorophenylsilane, ethyl cellulose and ethyl silicate is 3:2:2, the concentration of the trichlorophenylsilane in ether is 400g / L, the stirring speed for uniform stirring is 500r / min, the ultrasonic frequency of the ultrasonic dispersion is 100kHz, and the temperature is 20°C; the spraying speed is 8mL / min, the spraying atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 10:1, and the deposition temperature is 70°C; the solvent for soaking and drying is ethanol, and the drying temperature is 100°C; a2, soaking the porous silica particles in an acid solution for 2 hours, filtering and drying to obtain acidified silica particles, wherein the concentration of the porous silica particles in the acid solution is 400 g / L, the acid solution is a hydrochloric acid solution with a pH of 6, and the soaking temperature is 30°C; the drying temperature is 120°C; a3, dimethyldimethoxysilane is placed in ether to form a dilute solution, then the acidified silica is placed and a small amount of distilled water is added dropwise, the solution is subjected to ultrasonic treatment and filtered, and the modified porous silica particles are obtained by spray drying, wherein the concentration of the dimethyldimethoxysilane in the ether is 40 g / L, the concentration of the acidified silica in the ether is 300 g / L, the amount of distilled water added is 150% of the molar amount of the dimethyldimethoxysilane, the ultrasonic frequency of the ultrasonic treatment is 100 kHz, the temperature is 10°C, the atmosphere of the spray drying is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 10:1, and the temperature is 100°C.
[0039] The processing aid is ACR processing aid HF-401.
[0040] The lubricant is oxidized polyethylene wax.
[0041] The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 4:1.
[0042] The preparation method of the modified PVC heat shrinkable label film comprises the following steps:
[0043] Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry mix, the stirring speed is 3000 r / min, and the temperature is 10° C.;
[0044] Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 190° C.;
[0045] Step 3, after mixing PVC masterbatch, PETG and plasticizer, adding them into a single screw extruder for melt extrusion, and blowing them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 215° C., the water bath heating temperature before the two-bubble blowing is 89° C., and the two-bubble blowing ratio is 2.8; the PETG is ground before use.
[0046] Example 3
[0047] A method for preparing a modified PVC heat shrinkable label film, wherein the mass ratio of the label film is:
[0048] 100 parts of PVC resin, 20 parts of PETG, 0.35 parts of plasticizer, 4 parts of toughening agent, 4 parts of processing aid, 0.6 parts of lubricant, and 0.3 parts of stabilizer.
[0049] The plasticizer is 1-ethyl phosphate-3-methyl imidazolium chloride.
[0050] The toughening agent adopts modified silica, and the modified silica uses dimethylsilane as a branched structure and porous silica as a framework; the preparation method of the modified silica comprises the following steps: a1, adding trichlorophenylsilane, ethyl cellulose and ethyl silicate into ether and stirring evenly to form a mixed solution, spraying into a reaction kettle for deposition to form particles after ultrasonic dispersion, and obtaining porous silica particles by soaking and drying, wherein the molar ratio of the trichlorophenylsilane, ethyl cellulose and ethyl silicate is 2:1:2, the concentration of the trichlorophenylsilane in ether is 350g / L, the stirring speed for uniform stirring is 400r / min, the ultrasonic frequency of the ultrasonic dispersion is 90kHz, and the temperature is 15°C; the spraying speed is 6mL / min, the spraying atmosphere is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor is 9:1, and the deposition temperature is 65°C; the solvent for soaking and drying is ethanol, and the drying temperature is 95°C a2, soak the porous silica particles in an acid solution for 2 hours, filter and dry to obtain acidified silica particles, the concentration of the porous silica particles in the acid solution is 300 g / L, the acid solution uses a hydrochloric acid solution with a pH of 5, and the soaking temperature is 25°C; the drying temperature is 110°C; a3, put dimethyldimethoxysilane into ether to form a dilute solution, then put the acidified silica into it and add a small amount of distilled water, filter after ultrasonic treatment, and spray dry to obtain modified porous silica particles, the concentration of the dimethyldimethoxysilane in ether is 30 g / L, the concentration of the acidified silica in ether is 200 g / L, the amount of distilled water added is 140% of the molar amount of dimethyldimethoxysilane, the ultrasonic frequency of the ultrasonic treatment is 90 kHz, the temperature is 8°C, the atmosphere of the spray drying is a mixed atmosphere of nitrogen and water vapor, and the volume ratio of nitrogen to water vapor in the mixed atmosphere is 9:1, and the temperature is 95°C.
[0051] The processing aid is ACR processing aid HF-401.
[0052] The lubricant is oxidized polyethylene wax.
[0053] The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 3:1.
[0054] The preparation method of the modified PVC heat shrinkable label film comprises the following steps:
[0055] Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry blend, the stirring speed is 2500r / min, and the temperature is 8°C;
[0056] Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 165° C.;
[0057] Step 3, after mixing PVC masterbatch, PETG and plasticizer, adding them into a single screw extruder for melt extrusion, and blowing them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 185° C., the water bath heating temperature before the two-bubble blowing is 87° C., and the two-bubble blowing ratio is 2.6; the PETG is ground before use.
[0058] Example 4
[0059] A method for preparing a modified PVC heat shrinkable label film, wherein the mass ratio of the label film is:
[0060] 100 parts of PVC resin, 20 parts of PETG, 0.35 parts of plasticizer, 4 parts of toughening agent, 4 parts of processing aid, 0.6 parts of lubricant, and 0.3 parts of stabilizer.
[0061] The plasticizer is 1-ethyl phosphate-3-methyl imidazolium chloride.
[0062] The toughening agent is silicon dioxide.
[0063] The processing aid is ACR processing aid HF-401.
[0064] The lubricant is oxidized polyethylene wax.
[0065] The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 3:1.
[0066] The preparation method of the modified PVC heat shrinkable label film comprises the following steps:
[0067] Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry blend, the stirring speed is 2500r / min, and the temperature is 8°C;
[0068] Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 165° C.;
[0069] Step 3, after mixing PVC masterbatch, PETG and plasticizer, add them into a single screw extruder for melt extrusion, and blow them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 185°C, the water bath heating temperature before the two-bubble blowing is 87°C, and the two-bubble blowing ratio is 2.6; the PETG is ground before use
[0070] Comparative Example 1
[0071] Comparative Example 1 uses a commercially available PVC label film, model: 890*0.045*50%.
[0072] Performance Testing
[0073] The products of Examples 1-4 and the products of the comparative example were used as test samples to carry out performance tests.
[0074]
[0075] Among them, the low-temperature cracking test of the label film: a Nongfu Spring 500ml water bottle (bottle body diameter is 52mm, bottle mouth diameter is 30mm, bottle height is 230mm) filled with 500ml of water is used as the test bottle. The heat shrinkable label film is cut and folded to make a cylindrical sleeve label with a height (longitudinal shrinkage) of 200mm and a folded diameter (lateral shrinkage) of 163mm, and it is flattened and shrunk on the water bottle filled with water in a 100°C water bath. There are 10 samples in each group, and 3 groups are tested in each embodiment. Put the test bottle with the "label" in a constant low-temperature cabinet, take it out after leaving it for 8 hours, check the label one by one, and record the number of cracked labels. The total number of cracked labels in the 30 samples is the test value of the low-temperature cracking test of the label film.
[0076] The above data show that the comparison between Example 3 and Example 4 shows that the modified silica of the present technical solution can effectively improve the mechanical strength of the PVC heat shrinkable film and maintain the improvement of its own heat shrinkage rate. At the same time, the comparison between Examples 1-4 and the comparative example shows that the present technical solution can improve the problem of poor shrinkage rate of the PVC label film, and also improve the cold resistance problem of the PVC label film, thereby greatly improving the application scope of the PVC label film.
[0077] It is understood that the above specific description of the present invention is only used to illustrate the present invention and is not limited to the technical solutions described in the embodiments of the present invention. Those skilled in the art should understand that the present invention can still be modified or replaced by equivalents to achieve the same technical effects; as long as the use requirements are met, they are within the protection scope of the present invention.
Claims
1. A method for preparing a modified PVC heat shrinkable label film, Features: The mass ratio of the label film: 100 parts of PVC resin, 15-25 parts of PETG, 0.18-0.45 parts of plasticizer, 2-5 parts of toughening agent, 3-5 parts of processing aid, 0.5-0.7 parts of lubricant, and 0.2-0.4 parts of stabilizer.
2. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The plasticizer is an ionic liquid, specifically 1-ethyl phosphate-3-methylimidazolium chloride.
3. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The toughening agent is modified silicon dioxide.
4. The method for preparing the modified PVC heat shrinkage label film according to claim 3, Features: The modified silicon dioxide uses dimethylsilane as a branched structure and porous silicon dioxide as a framework.
5. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The processing aid is ACR processing aid HF-401.
6. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The lubricant is oxidized polyethylene wax.
7. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The stabilizer is a mixture of methyl tin sulfate and phosphite chelating agent J-1500, and the mass ratio of the two is 3-4:
1.
8. The method for preparing the modified PVC heat shrinkage label film according to claim 1, Features: The preparation method of the modified PVC heat shrinkable label film comprises the following steps: Step 1, putting PVC resin, toughening agent, processing aid, lubricant and stabilizer into a mixer and stirring to obtain a dry mix, the stirring speed is 2000-3000r / min, and the temperature is 5-10°C; Step 2, putting the dry blend into an extruder for granulation to obtain a PVC masterbatch, wherein the extruder is a single-screw extruder or a twin-screw extruder, and the extrusion temperature is 145-190° C.; Step 3, after mixing PVC masterbatch, PETG and plasticizer, adding them into a single screw extruder for melt extrusion, and blowing them twice to obtain a PETG modified PVC heat shrinkable label film; the temperature of the melt extrusion is 155-215° C., the water bath heating temperature before the second bubble blowing is 85-89° C., and the second bubble blowing ratio is 2.4-2.8; the PETG is ground before use.