Degradable high-toughness high-barrier container and preparation process thereof

Through the design of a three-layer composite material, combining bio-based polyurethane, silicon oxide film and cellulose acetate-chitosan composite film, the problem of insufficient strength and barrier properties of existing degradable materials in packaging containers is solved, and the problem of insufficient strength and barrier properties of existing degradable materials in packaging containers is achieved. High strength, toughness and excellent barrier properties, and achieve material degradation under specific conditions.

CN118930934APending Publication Date: 2024-11-12HUNAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411169710.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing biodegradable biopolymer materials cannot meet the requirements of high strength and toughness and high barrier properties in the packaging container field, especially the insufficient barrier properties of water and oxygen, which limits their application.

Method used

Design of a composite material with a three-layer structure, in which the inner layer is a bio-based polyurethane composite blow molding layer, a silicon oxide film layer in the middle, and a cellulose acetate-chitosan composite film, formed by vacuum sputtering and coating processes , combine nanoparticles and surface modifiers to improve material performance.

Benefits of technology

It achieves high strength, toughness and excellent water and oxygen barrier properties, and is printable, meets the comprehensive performance requirements of packaging containers, and realizes material degradation under specific conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930934A_ABST
    Figure CN118930934A_ABST
Patent Text Reader

Abstract

The invention relates to a degradable high-toughness high-barrier container and a preparation process thereof, and the container is formed by compounding three layers of structures, including an inner biopolyester composite blow molding layer, a middle silicon oxide film layer and an outer degradable covering film layer. Wherein the biopolyester composite blow molding layer is formed by injecting and blow molding bio-based polyurethane serving as a main raw material, a silicon oxide film layer is plated on the surface of the blow molding layer through vacuum sputtering, the blow molding layer is transferred into a treatment chamber after film plating, the surface of a container is sequentially coated with a coupling agent aqueous solution and a pre-polymerization solution, and the degradable covering film layer is obtained after curing; the container has excellent strength, toughness and water vapor and gas barrier property, and can be applied to the field of food and medicine packaging.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of polymer composite materials, and particularly relates to a degradable container with high strength, high toughness and high barrier properties, and a preparation method and application thereof. Background Art

[0002] Pure plastic resins such as PET are widely used in the preparation of blow-molded containers due to their good mechanical properties, processability and gas barrier properties. They are widely used in the fields of beverages, food dressings and industrial supplies. Although plastics have excellent performance, their non-degradability also brings a series of environmental and health problems. Finding packaging container materials that also have excellent performance and are degradable is still the direction of people's efforts.

[0003] In the process of people's search for high-strength, high-barrier biodegradable materials, biopolyesters such as polylactic acid (PLA) and polyhydroxyalkanoates (PHA) have been widely valued for their good strength and processability, but their barrier properties have never been able to meet the requirements of food containers. Various physical and chemical modifications have been used for exploration, such as adding nanoparticles and using a variety of biodegradable resin composites. Although their strength and toughness have been improved to varying degrees, their water and oxygen barrier properties cannot be substantially improved due to the intrinsic structural characteristics of biodegradable materials, which in turn limits their application in the field of packaging containers.

[0004] In the field of packaging, multi-layer composite is a common method to improve barrier properties. For example, Tetra Pak has achieved a significant improvement in barrier properties through multi-layer composite of paper, plastic, etc. Multi-layer co-extrusion, multi-layer composite of different structures such as PET / barrier layer / PET three-layer structure, "PET / barrier layer / PET / combination layer / PET" five-layer structure have also been used, and have good comprehensive performance. Using this method in the field of degradable packaging materials can solve the comprehensive problems of barrier properties and strength of materials to a certain extent. However, finding a suitable multi-layer structure that meets the requirements of strength and barrier and achieves good processing effects is undoubtedly still the key exploration direction in this field.

[0005] The patent of this invention combines the rational use of degradable materials and multi-layer composite technology to develop a packaging container with good strength and toughness, excellent barrier properties and printability, providing a high-quality option for degradable alternatives. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a degradable high-strength and high-barrier container and a preparation process thereof. The developed container has excellent ductility, tensile strength and water and oxygen barrier properties, and can be degraded under specific conditions.

[0007] The present invention is achieved by the following technical means: A degradable high-strength and high-barrier container, which is composed of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer.

[0008] Furthermore, the polyester composite blow molding layer comprises the following components and proportions: Bio-based polyurethane 100 Nanoparticles or organic hydrazide nucleating agent 0.5-1 Bio-based plasticizer 3.5-8 Furthermore, the nanoparticles are one of nano-silicon dioxide, nano-hydroxyapatite, nano-montmorillonite and nano-titanium dioxide, and the particle size is between 10-200nm.

[0009] Furthermore, the nanoparticles may be added after being surface-modified, such as by ionic surface modification or grafting modification.

[0010] Furthermore, the organic hydrazide nucleating agent is one of an aliphatic hydrazide nucleating agent and a phenylhydrazide nucleating agent, including but not limited to 1,4-naphthalene dicarboxylic acid dinicotinyl hydrazide, sebacic acid diphenyl dihydrazide, adipic acid dihydrazide, 3,4,5-trimethoxybenzohydrazide, aliphatic dicarboxylic acid dihydrazide, sebacic acid diphenyl dihydrazide, and stearic hydrazide.

[0011] Furthermore, the bio-based plasticizer is one of tri-n-butyl citrate, acetyl tributyl citrate, epoxidized soybean oil, epoxidized castor oil, and epoxidized linseed oil.

[0012] Furthermore, the bio-based polyurethane is prepared by reacting bio-based oligomer polyol, polyisocyanate, chain extender and cross-linking agent, and has a molecular weight between 200,000 and 400,000 and a melting point between 140 and 170°C.

[0013] Further, the bio-based polyurethane may be a commercially available product, such as eTPU-Bio2190, eTPU-Bio2195, eTPU-Bio2197, eTPU-Bio2190C of Shenzhen Guanghua Weiye Co., Ltd., BASF polyurethane Elastollan® N65AP, N65A12P, N75AP, N75A12P series, preferably, eTPU-Bio2197, eTPU-Bio2190C and Elastollan® N75AP, N75A12P series; Furthermore, the bio-based polyurethane can also be prepared by self-synthesis, and the bio-based oligomer polyol includes plant oil-based polyol, plant phenol polyol, wood fiber-based polyol, sugar-based polyol, such as soybean oil-based polyol, castor oil-based polyol; the polyisocyanate includes but is not limited to IPDI, TDI, PAPI, MDI, etc.; the chain extender and cross-linking agent are small molecule polyamines and polyols.

[0014] Further, the process of the biopolyester composite blow molding layer is as follows: (1) The components and a release agent having a mass fraction of 0.5-1% of bio-based polyurethane are mixed evenly, and then put into a screw extruder for extrusion and pelletization to obtain pellets, and then dried at 110-140° C. for 6-12 hours; (2) The pellets are put into an injection molding machine for injection molding to form a embryo body. The injection molding temperature is between 10-40°C above the melting point of the pellets, and the injection mold temperature is between 40-60°C; (3) The embryo is heated to a temperature between 5 and 10 °C above the Tg of the pellets, transferred to a mold, and blown by heated compressed air, with a transverse blow ratio of between 2.5 and 4 and a longitudinal blow ratio of between 4 and 6; the temperature of the heated compressed air is between 15 and 30 °C below the melting point of the pellets, and the mold temperature is between 80 and 110 °C; (4) After blow molding is completed, quickly lower the mold temperature to room temperature at a rate of 40-80℃ / min to complete demolding.

[0015] Furthermore, the processes (1) and (2) in the processing technology may also be: after drying the bio-based polyurethane at 110-140° C. for 6-12 hours, adding other components, mixing evenly and then directly injecting to form an embryo.

[0016] Furthermore, the intermediate silicon oxide film layer is obtained by vacuum sputtering on the surface of the polyester composite blow molding layer, and has a thickness of 20-50 μm.

[0017] Furthermore, the degradable covering film layer is a cellulose acetate-chitosan composite film, which uses cellulose acetate and chitosan as main raw materials and four-arm polyethylene glycol aldehyde as a crosslinking agent. It is formed by coating on the container surface and then drying and curing to form a film with a thickness between 25-80 μm.

[0018] Furthermore, the film thickness is related to the concentration of the coating prepolymer solution and the coating time.

[0019] Furthermore, the degree of substitution of the cellulose acetate is between 1.0-2.0; preferably, between 1.5-2.0.

[0020] Furthermore, the molecular weight of the four-arm polyhexanediol aldehyde group is between 2000-4000.

[0021] Furthermore, the coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a silane coupling agent aqueous solution with a mass concentration of 2-4%, add a small amount of formic acid to adjust the pH value to between 3-4, and stir until transparent; (2) The surface of the container covered with the silicon oxide film layer is evenly covered with the aqueous solution of silane coupling agent by spraying, dipping, brushing, etc., and then dried at 50-60° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is between 25% and 40%; the mass concentration of cellulose acetate is between 4% and 8%; and the mass concentration of chitosan is between 1.5% and 3%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 5-10%; (5) The surface-modified container is uniformly coated with prepolymer liquid A, and after drying, the prepolymer liquid B is contacted and coated, and then the prepolymer liquid B is dried and reacted at 50-80° C. for 2-4 minutes to obtain a cured outer layer of cellulose acetate-chitosan composite film.

[0022] Furthermore, the uniform coating of the prepolymer liquid A and the cross-linking liquid B can be carried out by brushing, spraying, rolling, or dipping; and the drying and heating can be carried out by physical heating or infrared heating.

[0023] Furthermore, the silane coupling agent is one of KH550, KH560 and KH570.

[0024] Furthermore, the degradable covering film layer may be printed after the surface is subjected to corona treatment.

[0025] Furthermore, the beneficial effects of the present invention are as follows: a three-layer composite structure is adopted, the inner layer structure ensures the strength and toughness, as well as the processability of the bottle body, and the formula and processing technology such as the blowing ratio ensure its good performance and a certain barrier effect; the coating of the middle layer mainly ensures its gas barrier property; the existence of the outer layer firstly ensures the integrity of the middle silicon oxide film layer, secondly plays a certain hydrophobic role, thirdly synergistically strengthens the mechanical properties of the container, and fourthly provides printability; in order to achieve good coating properties of the outer layer, multiple coating processes are adopted, and a coupling agent is introduced to achieve stable bonding between layers.

[0026] Further, the container material of the present invention is tested in the following manner: The tensile strength and elongation at break of container materials shall be tested according to GB / T 1040.3-2006 standard; The impact strength of container materials shall be tested according to GB / T 1043.1-2008 standard; The O2 barrier properties of container materials are tested according to GB / T 18454-2019 standard; The CO2 barrier properties of the container material shall be tested according to GB / T 1038.1-2022 standard; The water vapor barrier properties of container materials are tested according to GB / T 1037-2008 standard. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a flow chart of the preparation process of Example 1. DETAILED DESCRIPTION

[0028] The exemplary implementation methods of the present invention will be described in detail below, but these implementation methods are for exemplary purposes only and the present invention is not limited thereto. Example 1

[0029] A degradable high-strength and high-barrier container, the container is composed of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer. The preparation process is as follows Figure 1 shown.

[0030] The polyester composite blow molding layer comprises the following components and proportions: Bio-based polyurethane 100 Nano silicon dioxide 0.8 Tri-n-butyl citrate 6.5 The average particle size of the nano silicon dioxide is 40 nm, and the surface is modified by silane to improve its dispersibility.

[0031] The bio-based polyurethane is the eTPU-Bio2190C series of Shenzhen Guanghua Weiye Co., Ltd., with a melting point of 142°C.

[0032] The process of the biopolyester composite blow molding layer is as follows: (1) The above-mentioned bio-based polyurethane, surface-modified nano-silica, tri-n-butyl citrate, and a release agent in an amount of 0.8% by weight of the bio-based polyurethane are mixed evenly, and then put into a screw extruder for extrusion and pelletization to obtain pellets, which are then dried at 120° C. for 8 hours; (2) The pellets are put into an injection molding machine for injection molding to form a embryo body. The injection molding temperature is 160°C and the injection mold temperature is 50°C. (3) The embryo body is heated to 80°C, transferred to the mold, and blown by compressed air heated at 120°C, with a transverse blow ratio of 3.2, a longitudinal blow ratio of 5.6, and a mold temperature of 100°C; (4) After blow molding is completed, the mold temperature is quickly lowered to room temperature at a rate of 40°C / min to complete demolding.

[0033] The intermediate silicon oxide film layer is obtained on the surface of the polyester composite blow molding layer by vacuum sputtering and has a thickness of 40 μm.

[0034] The degradable covering film layer is a cellulose acetate-chitosan composite film, which is made of cellulose acetate and chitosan as main raw materials and four-arm polyhexanediol aldehyde as a crosslinking agent. The film is formed by a surface coating and then drying and curing process, and the film thickness is 45 μm.

[0035] The cellulose acetate is cellulose diacetate, and the degree of substitution is 1.6.

[0036] The molecular weight of the four-arm polyhexanediol aldehyde group is 3500.

[0037] The coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a 3.5% KH570 aqueous solution, add a small amount of formic acid to adjust the pH value to 3.5, and stir until transparent and uniform; (2) The surface of the container covered with the silicon oxide film layer is evenly covered with an aqueous solution of a silane coupling agent by spraying, and then dried at 55° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is 30%; the mass concentration of cellulose acetate is 6.5%; and the mass concentration of chitosan is 2.5%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 8%; (5) The surface modified container is uniformly covered with prepolymer liquid A by immersion, and after drying, it is contacted with and covered with cross-linking liquid B by immersion, and then the water is dried and reacted at 70°C for 3 minutes to obtain a cured outer layer of cellulose acetate-chitosan composite film.

[0038] The properties of the prepared container materials are shown in Table 1.

[0039] Example 2 A degradable high-strength and high-barrier container, which consists of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer.

[0040] The polyester composite blow molding layer comprises the following components and proportions: Bio-based polyurethane 100 Nano Titanium Dioxide 0.6 Epoxy castor oil 5.5 The average particle size of the nano titanium dioxide is 60 nm, and PMMA nano titanium dioxide is grafted on the surface.

[0041] The bio-based polyurethane is the eTPU-Bio2195 series of Shenzhen Guanghua Weiye Co., Ltd., with a melting point of 135°C.

[0042] The process of the biopolyester composite blow molding layer is as follows: (1) The above-mentioned bio-based polyurethane, surface-grafted PMMA nano-titanium dioxide, epoxy castor oil, and a release agent in an amount of 0.6% by weight of the bio-based polyurethane are mixed evenly, and then put into a screw extruder for extrusion and pelletization to obtain pellets, which are then dried at 120° C. for 8 hours; (2) The pellets are put into an injection molding machine for injection molding to form a embryo body. The injection molding temperature is 150°C and the injection mold temperature is 55°C. (3) The embryo body is heated to 75°C, transferred to the mold, and blow-molded by compressed air heated at 120°C, with a transverse blow ratio of 3.4, a longitudinal blow ratio of 5.4, and a mold temperature of 90°C; (4) After blow molding is completed, the mold temperature is quickly lowered to room temperature at a rate of 50°C / min to complete demolding.

[0043] The intermediate silicon oxide film layer is obtained on the surface of the polyester composite blow molding layer by vacuum sputtering and has a thickness of 35 μm.

[0044] The degradable covering film layer is a cellulose acetate-chitosan composite film, which uses cellulose acetate and chitosan as main raw materials and four-arm polyhexanediol aldehyde as a crosslinking agent. The film is formed by a surface coating and then drying and curing process, and the film thickness is between 45 μm.

[0045] The cellulose acetate is cellulose diacetate, and the degree of substitution is 1.8.

[0046] The molecular weight of the four-arm polyhexanediol aldehyde group is 3200.

[0047] The coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a 3% KH560 aqueous solution, add a small amount of formic acid to adjust the pH value to 3.5, and stir until transparent and uniform; (2) The surface of the container covered with the silicon oxide film layer is evenly covered with an aqueous solution of a silane coupling agent by spraying, and then dried at 55° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is 32%; the mass concentration of cellulose acetate is 6%; and the mass concentration of chitosan is 2.2%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 6.5%; (5) The surface-modified container is uniformly covered with prepolymer liquid A by rolling, and after drying, the prepolymer liquid B is contacted and covered by immersion, and then the prepolymer liquid B is dried and reacted at 80°C for 2 minutes to obtain a cured outer layer of cellulose acetate-chitosan composite film.

[0048] The properties of the prepared container materials are shown in Table 1.

[0049] Example 3 A degradable high-strength and high-barrier container, which consists of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer.

[0050] The polyester composite blow molding layer comprises the following components and proportions: Bio-based polyurethane 100 Nano-montmorillonite 0.6 Epoxidized soybean oil 7.0 The average particle size of the nano-montmorillonite is 40 nm, and the surface is modified by anions.

[0051] The bio-based polyurethane is BASF polyurethane Elastollan® N75A12P, which has a melting point of about 150°C.

[0052] The process of the biopolyester composite blow molding layer is as follows: (1) The above-mentioned bio-based polyurethane, anionic surface-modified nano-montmorillonite, epoxy soybean oil, and a release agent in an amount of 0.7% by weight of the bio-based polyurethane are mixed evenly, put into a screw extruder, extruded and pelletized to obtain pellets, and dried at 110° C. for 10 hours; (2) The pellets are placed in an injection molding machine for injection molding to form a body, the injection molding temperature is 165°C, and the injection mold temperature is 45°C; (3) The embryo body is heated to 80°C, transferred to the mold, and blown by compressed air heated at 125°C, with a transverse blow ratio of 3.8, a longitudinal blow ratio of 4.6, and a mold temperature of 100°C; (4) After blow molding is completed, the mold temperature is quickly lowered to room temperature at a rate of 50°C / min to complete demolding.

[0053] The intermediate silicon oxide film layer is obtained on the surface of the polyester composite blow molding layer by vacuum sputtering and has a thickness of 45 μm.

[0054] The degradable covering film layer is a cellulose acetate-chitosan composite film, which is made of cellulose acetate and chitosan as main raw materials and four-arm polyhexanediol aldehyde as a crosslinking agent, and is formed by a surface coating and then drying and curing process, and the film thickness is 60 μm.

[0055] The cellulose acetate is cellulose diacetate, and the degree of substitution is 1.8.

[0056] The molecular weight of the four-arm polyhexanediol aldehyde group is 3600.

[0057] The coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a 3.5% KH570 aqueous solution, add a small amount of formic acid to adjust the pH value to 4, and stir until transparent and uniform; (2) The surface of the container covered with the silicon oxide film layer is evenly covered with an aqueous solution of a silane coupling agent by spraying, and then dried at 55° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is 28%; the mass concentration of cellulose acetate is 5%; and the mass concentration of chitosan is 1.8%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 8%; (5) The surface modified container is uniformly covered with prepolymer liquid A by spraying, and after drying, the prepolymer liquid A is contacted and covered by immersion in cross-linking liquid B, and then the prepolymer liquid A is dried and reacted at 70°C for 3 minutes to obtain a cured outer layer of cellulose acetate-chitosan composite film.

[0058] The properties of the prepared container materials are shown in Table 1.

[0059] Example 4 A degradable high-strength and high-barrier container, which is composed of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer. The polyester composite blow-molded layer contains the following components and proportions: Bio-based polyurethane 100 Sebacic acid diphenyl dihydrazide 0.8 Epoxidized soybean oil 6.5 The bio-based polyurethane is BASF polyurethane Elastollan® 2190C, which has a melting point of about 145°C.

[0060] The process of the biopolyester composite blow molding layer is as follows: (1) The bio-based polyurethane was dried at 110° C. for 8 hours, and then diphenyl dihydrazide sebacic acid, epoxy soybean oil, and a release agent of 0.8% by weight of the bio-based polyurethane were added, mixed evenly, and then injected into an injection molding machine to form an embryo body. The injection molding temperature was 165° C. and the injection mold temperature was 60° C.; (3) The embryo body is heated to 75°C, transferred to the mold, and blown by compressed air heated at 130°C, with a transverse blow ratio of 3.5, a longitudinal blow ratio of 5.5, and a mold temperature of 95°C; (4) After blow molding is completed, the mold temperature is quickly lowered to room temperature at a rate of 45°C / min to complete demolding.

[0061] The intermediate silicon oxide film layer is obtained on the surface of the polyester composite blow molding layer by vacuum sputtering and has a thickness of 40 μm.

[0062] The degradable covering film layer is a cellulose acetate-chitosan composite film, which is made of cellulose acetate and chitosan as main raw materials and four-arm polyhexanediol aldehyde as a crosslinking agent. The film is formed by a surface covering and then drying and curing process, and the film thickness is 65 μm.

[0063] The cellulose acetate is cellulose diacetate, and the degree of substitution is 1.9.

[0064] The molecular weight of the four-arm polyhexanediol aldehyde group is 3800.

[0065] The coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a 3.0% KH560 aqueous solution, add a small amount of formic acid to adjust the pH value to 3.5, and stir until transparent and uniform; (2) The surface of the container covered with the silicon oxide film layer is evenly covered with an aqueous solution of a silane coupling agent by spraying, and then dried at 50° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is 32%; the mass concentration of cellulose acetate is 6.5%; and the mass concentration of chitosan is 2.2%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 7%; (5) The surface modified container is uniformly covered with prepolymer liquid A by spraying, and after drying, the prepolymer liquid A is contacted and covered by immersion in cross-linking liquid B, and then the prepolymer liquid A is dried and reacted at 75°C for 2.5 minutes to obtain a cured outer layer cellulose acetate-chitosan composite film.

[0066] The properties of the prepared container materials are shown in Table 1.

[0067] Comparative Example 1 Compared with Example 1, the surface of the polyester composite blow-molded layer is not covered with a silicon oxide film layer and a degradable covering film layer.

[0068] The properties of the prepared container materials are shown in Table 1.

[0069] Comparative Example 2 Compared with Example 1, the surface of the polyester composite blow-molded layer is not covered with a silicon oxide film layer, but is directly covered with a degradable covering film layer. Due to differences in the process, the thickness of the degradable covering film layer is 45 μm.

[0070] The properties of the prepared container materials are shown in Table 1.

[0071] Comparative Example 3 Compared with Example 1, Hisun REVODE 201 polylactic acid was used to replace bio-based polyurethane. Due to the difference in physical properties, the process conditions for processing into containers were changed accordingly, and other processes remained unchanged.

[0072] The processing technology of polyester composite blow molding layer is as follows: (1) Polylactic acid, surface-modified nano-silica, tri-n-butyl citrate, and a release agent in an amount of 0.8% by weight of polylactic acid are mixed evenly, and then put into a screw extruder for extrusion and pelletization to obtain pellets, which are then dried at 120° C. for 8 hours; (2) The pellets are put into an injection molding machine for injection molding to form a embryo body. The injection molding temperature is 220°C and the injection mold temperature is 60°C. (3) The embryo body is heated to 90°C, transferred to the mold, and blown by compressed air heated at 140°C, with a transverse blow ratio of 2.7, a longitudinal blow ratio of 3.5, and a mold temperature of 120°C; (4) After blow molding is completed, the mold temperature is quickly lowered to room temperature at a rate of 40°C / min to complete demolding.

[0073] The thickness of the intermediate silicon oxide film layer is 40 μm.

[0074] The thickness of the degradable covering film layer is 44 μm.

[0075] The properties of the prepared container materials are shown in Table 1.

[0076] Table 1. Material properties of containers prepared in Examples and Comparative Examples Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Tensile strength (MPa) 47.6 42.4 51.3 46.3 42.8 39.7 35.8 Elongation at break (%) 89.2 103.4 72.7 96.4 83.9 83.8 25.8 Impact strength (kJ / m²) 34.6 36.7 40.5 31.9 30.9 33.9 21.9 <![CDATA[O2 transmission rate cm 3 / (m 3 ·24 hr·MPa)]]> 32.6 33.8 35.2 45.8 872.7 643.7 93.4 <![CDATA[CO2 permeance cm 3 / (m 3 ·24 h·MPa)]]> 42.5 60.9 53.5 66.8 1048.1 731.9 132.9 <![CDATA[Water vapor transmission rate, g / (m 2 ·24hr·MPa) (25 μm thickness, 23 °C, 85 % humidity)]]> 23.6 24.7 39.5 44.3 406.1 297.5 35.4

Claims

1. A degradable high-strength and high-barrier container, which is composed of a three-layer composite structure, including an inner polyester composite blow-molded layer, a middle silicon oxide film layer and an outer degradable covering film layer.

2. The degradable high-strength and high-barrier container according to claim 1, characterized in that: The biopolyester composite blow molding layer comprises the following components and proportions: Bio-based polyurethane 100 Nanoparticles or organic hydrazide nucleating agent 0.5-1 Bio-based plasticizer 3.5-8 The nanoparticles are one of nano-silicon dioxide, nano-hydroxyapatite, nano-montmorillonite and nano-titanium dioxide, and the particle size is between 10-200nm; the organic hydrazide nucleating agent is one of aliphatic hydrazide nucleating agent and phenylhydrazide nucleating agent; the bio-based plasticizer is one of tri-n-butyl citrate, acetyl tributyl citrate, epoxidized soybean oil, epoxidized castor oil and cyclolinazone.

3. The degradable high-strength and high-barrier container according to claim 1, characterized in that: The bio-based polyurethane is prepared by reacting bio-based oligomer polyol, polyisocyanate, chain extender and cross-linking agent, and has a molecular weight between 200,000 and 400,000.

4. The degradable high-strength and high-barrier container according to claims 1 and 2, characterized in that: The process of the biopolyester composite blow molding layer is as follows: (1) The raw materials in claim 2 and a release agent with a mass fraction of 0.5-1% of bio-based polyurethane are mixed evenly, and then put into a screw extruder for extrusion and pelletization to obtain pellets, and then dried at 110-140° C. for 6-12 hours; (2) The pellets are put into an injection molding machine for injection molding to form a embryo body. The injection molding temperature is between 10-40°C above the melting point of the pellets, and the injection mold temperature is between 40-60°C; (3) The embryo is heated to a temperature between 5 and 10 °C above the Tg of the pellets, transferred to a mold, and blown by heated compressed air, with a transverse blow ratio of between 2.5 and 4 and a longitudinal blow ratio of between 4 and 6; the temperature of the heated compressed air is between 15 and 30 °C below the melting point of the pellets, and the mold temperature is between 80 and 110 °C; (4) After blow molding is completed, quickly lower the mold temperature to room temperature at a rate of 40-80℃ / min to complete demolding.

5. The degradable high-strength and high-barrier container according to claim 4, characterized in that: The processes (1) and (2) in the processing technology may also be: after drying the bio-based polyurethane at 110-140° C. for 6-12 hours, adding other components, mixing evenly and then directly injecting to form an embryo.

6. The degradable high-strength and high-barrier container according to claim 1, characterized in that: The intermediate silicon oxide film layer is obtained by vacuum sputtering on the surface of the biopolyester composite blow molding layer, and has a thickness of 20-50 μm.

7. The degradable high-strength and high-barrier container according to claim 1, characterized in that: The degradable covering film layer is a cellulose acetate-chitosan composite film, which uses cellulose acetate and chitosan as main raw materials and four-arm polyethylene glycol aldehyde as a crosslinking agent. It is formed by drying and curing after coating on the container surface, and the film thickness is between 25-80 μm.

8. The degradable high-strength and high-barrier container according to claim 7, characterized in that: The coating process of the cellulose acetate-chitosan composite film is as follows: (1) Prepare a silane coupling agent aqueous solution with a mass concentration of 2-4%, add a small amount of formic acid to adjust the pH value to between 3-4, and stir until it is uniform and transparent; (2) The surface of the container covered with the silicon oxide film layer is uniformly coated with an aqueous solution of a silane coupling agent by spraying, dipping, brushing, etc., and then dried at 50-60° C. until the water evaporates to obtain a surface-modified container; (3) dissolving cellulose acetate and chitosan in a formic acid aqueous solution and stirring to obtain a prepolymer solution A; wherein the volume concentration of the formic acid aqueous solution is between 25% and 40%; the mass concentration of cellulose acetate is between 4% and 8%; and the mass concentration of chitosan is between 1.5% and 3%; (4) dissolving the four-arm polyhexanediol aldehyde group in pure water to prepare a cross-linking solution B with a mass concentration of 5-10%; (5) The surface modified container is uniformly coated with prepolymer liquid A, and after drying, the prepolymer liquid B is contacted and coated, and the prepolymer liquid B is dried and reacted at 50-80° C. for 2-4 minutes to obtain a cured outer layer of cellulose acetate-chitosan composite film.

9. The degradable high-strength and high-barrier container according to claim 1, characterized in that: The degree of substitution of the cellulose acetate is between 1.0 and 2.

0.

10. The degradable high-strength and high-barrier container according to claims 1 and 5, characterized in that: The silane coupling agent is one of KH550, KH560 and KH570.