Conductive foamed polypropylene bead, preparation method thereof and molded part
By introducing special melting fingers and melting points into conductive EPP materials, the problem of high steam molding pressure of traditional conductive EPP materials is solved, and more stable molding performance and surface resistance are achieved, and the forming pressure is reduced. , improving the application value of the product and energy conservation and emission reduction effects.
Patent Information
- Application Number
- CN202411191265.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional conductive EPP materials have high pressure during steam molding, resulting in unstable molding and material strength loss, and changes in foaming conditions increase production risks.
Using the process optimization of the conductive masterbatch combination with special melting fingers and melting point, conductive EPP foam beads with stable surface resistance and wide foaming windows are prepared to reduce steam by coextrusion equipment and supercritical carbon dioxide press foaming process. Molding pressure.
It significantly reduces the steam molding pressure, improves molding performance and surface resistance stability, enhances the application value of the product and energy-saving and emission reduction effects.
Smart Images

Figure BDA0005015173640000071 
Figure BDA0005015173640000081 
Figure BDA0005015173640000082
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of functional foaming materials, in particular to a conductive foamed polypropylene bead and a preparation method and a molded product thereof. Background Art
[0002] During the use of electronic equipment, due to the electromagnetic interference from the surrounding environment, the electronic equipment may become unstable or even malfunction. Semi-conductive shielding materials can shield electromagnetic wave signals outside the equipment by absorption, reflection, scattering, etc. to prevent them from affecting the equipment. Its protective effect can not only prevent the failure of electronic equipment, but also reduce the impact of electromagnetic radiation on personnel and the environment. Semi-conductive shielding materials can be divided into conductive shielding materials and insulating shielding materials according to their characteristics. Among them, conductive shielding materials are the most common. They are widely used in electronic communications, aerospace, medical equipment and other equipment, as well as in ensuring the stable operation of high-precision and high-stability equipment. They can protect the equipment from the influence of electromagnetic interference in electronic equipment.
[0003] Polypropylene foam material (EPP for short) has been developing rapidly in recent years due to its lightweight, high strength and steam molding characteristics. It has good use cases in automobiles, packaging, furniture and aerospace. With the in-depth promotion of environmental protection issues by the country, EPP materials have shown new application prospects in more and more industries. At present, the annual use of EPP in China is 80,000-100,000 tons / year, and it is increasing at a rate of 15% per year.
[0004] Conductive EPP foamed polypropylene material refers to the EPP foamed beads obtained through the design of formula and improvement of foaming process on the basis of the original EPP. After steam molding, it has certain surface resistance characteristics. According to different resistance values, it can be subdivided into high conductive, semi-conductive and antistatic products. It has certain application prospects in electrical packaging, electronic components transportation and microwave darkrooms.
[0005] The preparation of traditional conductive EPP is to add a large amount of conductive carbon black into the formula, and then obtain EPP foam material with conductive properties through a foaming process. Although its electrical performance meets the standards, the addition of a large amount of conductive carbon black will cause carbon black accumulation, which greatly reduces the fluidity of the raw material and greatly increases its steam molding pressure. Summary of the invention
[0006] In order to solve the problem of high steam molding pressure of conductive EPP in the prior art, the present invention provides a method for preparing conductive foamed polypropylene beads. The preparation method can obtain energy-saving conductive EPP foamed beads with stable surface resistance and a wider foaming window by introducing a conductive masterbatch with a special melting point and a melting point, combined with process optimization. The steam molding pressure can be significantly reduced, thus solving the problem of high steam molding pressure of conductive EPP in the prior art.
[0007] The technical solution adopted by the present invention to solve its technical problem is:
[0008] A method for preparing conductive foamed polypropylene beads comprises the following steps:
[0009] S1: According to the formula, the polypropylene base material α and the conductive carbon black C are blended in an internal mixer, and then granulated by twin-screw extrusion to obtain a conductive masterbatch γ;
[0010] The polypropylene base material α has a melting point range of 125°C-130°C and a melt index range of 20-80 (g / 10min / 220°C);
[0011] S2: Blending polypropylene base material A, dispersant B, conductive carbon black C and carbon black D in an internal mixer, and then extruding and granulating through a twin-screw device to obtain a black masterbatch β;
[0012] S3: Using a co-extrusion device, the conductive masterbatch γ is used as the skin layer, and the polypropylene base material A, the black masterbatch β, the nucleating agent E, the lubricant F, and the stabilizer G are used as the core layer, and the mixture is blended, drawn, and granulated to obtain conductive polypropylene pre-foamed particles;
[0013] S4: foaming the conductive polypropylene pre-foamed particles through a supercritical carbon dioxide autoclave pressure foaming process to obtain conductive polypropylene foamed beads.
[0014] Optionally, step S4 further includes: secondary foaming of the conductive polypropylene foam beads by a steam foaming process.
[0015] Optionally, the preparation method of the polypropylene base material α is as follows: compounding a polypropylene raw material H and a polypropylene raw material I, and adding a dispersant B to obtain a polypropylene base material α; wherein the melting point range of the polypropylene raw material H is 115°C-125°C; and the melt index of the polypropylene raw material I is 100-200 (g / 10min / 220°C).
[0016] Optionally, in the polypropylene base material α, the mass fraction of the polypropylene raw material I is 3%-6%, and the mass fraction of the dispersant B is 2%.
[0017] Optionally, in step S1, the mass ratio of the polypropylene base material α to the conductive carbon black C is (9-7): (1-3).
[0018] Optionally, the particle size of the conductive carbon black C is 200-500 nm.
[0019] Optionally, the polypropylene base material A is a random copolymer polypropylene with a melting point of 145-155° C. and a melt index of 5-15 (g / 10min / 220° C.).
[0020] Optionally, the dispersant B is ethylene bisstearamide.
[0021] Optionally, the particle size of the carbon black D is 50-200 nm.
[0022] Optionally, in step S2, the mass ratio of the polypropylene base material A, the dispersant B, the conductive carbon black C and the carbon black D is (35-53): (2-5): (5-10): (40-50).
[0023] Optionally, the mass ratio of the polypropylene base material A, the black masterbatch β, the nucleating agent E, the lubricant F, and the stabilizer G in the core layer of step S3 is (81.7-88.4): (10-15): (0.1-0.3): (1-2): (0.5-1).
[0024] Another object of the present invention is to provide conductive foamed polypropylene beads, which are prepared by the method for preparing conductive foamed polypropylene beads as described above.
[0025] Another object of the present invention is to provide a molded article obtained by steam molding the conductive foamed polypropylene beads as described above.
[0026] The beneficial effects of the present invention are:
[0027] The preparation method of the conductive foamed polypropylene beads provided by the present invention combines the characteristics of the material itself, especially the conductive masterbatch α, with its special melting point and melting point. Under the condition of maintaining a certain gap with the melting point of the core layer, the product is given better molding performance, more stable surface resistance, and a certain reduction advantage in molding pressure. The stability and subsequent application design of multiple products have good use value, and energy-saving conductive EPP foamed beads with stable surface resistance and a wider foaming window can be obtained. The steam molding pressure can be significantly reduced, and better contributions are made to energy conservation and emission reduction. DETAILED DESCRIPTION
[0028] The present invention is now further described in detail. The embodiments described below are exemplary and intended to be used to explain the present invention, but cannot be understood as limiting the present invention. All other embodiments obtained by ordinary technicians in this field without creative work based on the embodiments of the present invention belong to the scope of protection of the present invention.
[0029] In the preparation of traditional conductive EPP, the introduction of excessive carbon black will not only greatly increase its steam molding pressure, but also cause a certain loss in the strength of the foam itself. In addition, it will change the foaming conditions of the material, and the foaming back pressure will be significantly increased, which will pose a certain risk to production stability.
[0030] In order to solve the problem of high steam molding pressure of conductive EPP in the prior art, the present invention provides a method for preparing conductive foamed polypropylene beads, which comprises the following steps:
[0031] S1: According to the formula, the polypropylene base material α and the conductive carbon black C are blended in an internal mixer, and then granulated by twin-screw extrusion, and dried for standby use to obtain a conductive masterbatch γ; wherein the melting point range of the polypropylene base material α is 125°C-130°C, and the melt index range is 20-80 (g / 10min / 220°C); preferably, the internal mixing processing temperature in this step is 150-180°C; the twin-screw processing temperature is 180-220°C, the pelletizing size is 30-40mg, the length is 4-8mm, and the drying temperature is 80°C for 6h;
[0032] S2: Blending polypropylene base material A, dispersant B, conductive carbon black C and carbon black D through an internal mixer, extruding and granulating through a twin-screw device, and drying for standby use to obtain a black masterbatch β; preferably, the internal mixing temperature in this step is 150-180°C; the twin-screw processing temperature is 180-220°C, the pelletizing size is 30-40mg, the length is 4-8mm, and the drying temperature is 80°C for 6h;
[0033] S3: Using a co-extrusion device, the conductive masterbatch γ is used as the skin layer, and the polypropylene base material A, black masterbatch β, nucleating agent E, lubricant F, and stabilizer G are used as the core layer, and the co-extrusion device is adjusted to obtain conductive polypropylene pre-foamed particles with conductive properties.
[0034] Preferably, in this step, the nucleating agent E is zinc borate or silicon dioxide, the lubricant F is oleamide or erucamide, and the stabilizer G is a mixture of antioxidant 1010 and light stabilizer 622 in a mass ratio of 1:1; preferably, the processing temperature of the core layer is 180-220°C, the processing temperature of the skin layer conductive masterbatch is 200-240°C, the ratio of the skin layer extrusion speed to the core layer extrusion speed is (0.5-2): (9.5-8), the skin layer thickness is 10-20% of the total thickness of the conductive polypropylene pre-foamed particles, and the wire drawing pelletizing size is 2 mm long and weighs 1 mg;
[0035] S4: After the conductive polypropylene pre-foamed particles are mixed with water, kaolin and butter by a supercritical carbon dioxide autoclave foaming process, the mixture is heated to a certain temperature and pressure, and then the pressure is released and the temperature is lowered to foam the mixture to obtain conductive polypropylene foam beads; preferably, in the foaming of the conductive polypropylene pre-foamed particles in this step, the water-to-material ratio is 2:1-5:1, the foaming temperature is 148-155°C, and the foaming pressure is 1.8-2.5MPa; in the foaming of the conductive polypropylene pre-foamed particles, the amount of kaolin and butter added is 0.5-1% of the mass of water.
[0036] The preparation method of the conductive foamed polypropylene beads provided by the present invention combines the characteristics of the material itself, especially the conductive masterbatch α, with its special melting point and melting point. Under the condition of maintaining a certain gap with the melting point of the core layer, the product is given better molding performance, more stable surface resistance, and a certain reduction advantage in molding pressure. The stability and subsequent application design of multiple products have good use value, and energy-saving conductive EPP foamed beads with stable surface resistance and a wider foaming window can be obtained. The steam molding pressure can be significantly reduced, and better contributions are made to energy conservation and emission reduction.
[0037] In the method for preparing the conductive foamed polypropylene beads, the step S4 further comprises: performing secondary foaming on the conductive polypropylene foamed beads by a steam foaming process to obtain conductive polypropylene foamed beads with a lighter density.
[0038] The preparation method of the polypropylene base material α in the preferred step S1 of the present invention is as follows: compounding a polypropylene raw material H and a polypropylene raw material I, and adding a dispersant B to obtain a polypropylene base material α; wherein the melting point range of the polypropylene raw material H is 115°C-125°C; the melt index of the polypropylene raw material I is 100-200 (g / 10min / 220°C); and the dispersant B is ethylene bisstearamide.
[0039] In the preferred polypropylene base material α of the present invention, that is, in the raw materials for preparing the polypropylene base material α, the mass fraction of the polypropylene raw material I is 3%-6%, and the mass fraction of the dispersant B is 2%.
[0040] The invention selects a polypropylene raw material with a melting point between 115°C and 125°C, and compounding is performed by adding 3% to 6% by mass of a high melt index polypropylene raw material (melt index 100-200 (g / 10min / 220°C)), and simultaneously adding 2% by mass of an EBS (ethylene bisstearamide) dispersant to obtain a polypropylene base material α with a melting point between 125°C and 130°C and a melt index between 20-80 (g / 10min / 220°C).
[0041] In order to take into account both the conductive properties and the mechanical properties, the mass ratio of the polypropylene base material α to the conductive carbon black C in step S1 is preferably (9-7): (1-3); and the particle size of the conductive carbon black C is preferably 200-500 nm.
[0042] Specifically, the preferred polypropylene base material A of the present invention is random copolymer polypropylene with a melting point of 145-155°C and a melt index of 5-15 (g / 10min / 220°C); the preferred dispersant B is ethylene bisstearamide (EBS); and the carbon black D is conventional carbon black with a particle size of 50-200nm.
[0043] Preferably, the mass ratio of the polypropylene base material A, the dispersant B, the conductive carbon black C and the carbon black D in step S2 is (35-53): (2-5): (5-10): (40-50).
[0044] Preferably, the mass ratio of the polypropylene base material A, the black masterbatch β, the nucleating agent E, the lubricant F and the stabilizer G in the core layer of step S3 is (81.7-88.4): (10-15): (0.1-0.3): (1-2): (0.5-1).
[0045] Another object of the present invention is to provide conductive foamed polypropylene beads, which are prepared by the method for preparing conductive foamed polypropylene beads as described above.
[0046] The conductive foamed polypropylene beads provided by the present invention have better molding performance, more stable surface resistance, and a certain advantage of reduced molding pressure.
[0047] Another object of the present invention is to provide a molded article, which is obtained by steam molding the conductive foamed polypropylene beads as described above.
[0048] In the preferred molding process of the present invention, after the product is pre-pressed (maintaining pressure 2.5-4kg), it is molded by a steam molding machine with a molding pressure of 0.2-0.3MPa, and the molded product is dried at 80°C for 6h to obtain a molded product of conductive polypropylene foam beads.
[0049] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, specific embodiments of the present invention are described in detail below.
[0050] Unless otherwise specified, the polypropylene base material α in each embodiment of the present invention and the comparative example is prepared according to the following method:
[0051] A polypropylene raw material H with a melting point of 120°C and a melt index of 10 (g / 10min / 220°C) was selected, and compounded by adding 5% by mass of a high melt index polypropylene raw material I (melting point of 160°C, melt index of 60 (g / 10min / 220°C)), and at the same time adding 2% by mass of an EBS (ethylene bisstearamide) dispersant to obtain a polypropylene base material α with a melting point of 130°C and a melt index of 20 (g / 10min / 220°C).
[0052] The formula of the conductive masterbatch γ in each embodiment of the present invention and the comparative example is shown in Table 1:
[0053] Table 1
[0054]
[0055]
[0056] In the preparation step of the conductive masterbatch γ, the mixing processing temperature is 170°C; the twin-screw processing temperature is 200°C, the pellet size is 30-40mg, the length is 6mm, and the drying temperature is 80°C for 6h.
[0057] The formula of black masterbatch β in each embodiment of the present invention and the comparative example is shown in Table 2:
[0058] Table 2
[0059] β-1 β-2 Polypropylene base material A (parts by weight) 53 35 Dispersant B 2 5 Conductive carbon black C 5 10 Conventional Carbon Black D 40 50
[0060] In the preparation step of black masterbatch β, the mixing temperature is 170°C; the twin-screw processing temperature is 200°C, the pelletizing size is 30-40mg, the length is 6mm, the drying temperature is 80°C, and the drying time is 6h; the polypropylene base material A is a random copolymer polypropylene with a melting point of 150°C and a melt index of 10 (g / 10min / 220°C); the dispersant B is ethylene bisstearamide (EBS); the particle size of the conductive carbon black C is 300nm; and the particle size of the conventional carbon black D is 150nm.
[0061] The formula of the conductive polypropylene pre-foamed particles in each embodiment is shown in Table 3:
[0062] Table 3
[0063]
[0064] The processing temperature of the core layer is 200°C, the processing temperature of the skin layer is 200°C, the ratio of the extrusion speed of the skin layer to the extrusion speed of the core layer is 1:9, the drawing pellet size is 2 mm long and weighs 1 mg; the polypropylene base material A is a random copolymer polypropylene with a melting point of 150°C and a melt index of 10 (g / 10min / 220°C); the nucleating agent E is zinc borate; the lubricant F is oleic acid amide; the stabilizer G is a mixture of antioxidant 1010 and light stabilizer 622 in a mass ratio of 1:1.
[0065] The pre-foamed particles prepared in the above embodiments were foamed, and the foaming parameters and performance test data are shown in Table 4:
[0066] Table 4
[0067]
[0068] In the above Table 4, "1-1" and "1-2" are both foamed with the pre-foamed particles prepared in Example 1; "2-1" and "2-2" are both foamed with the pre-foamed particles prepared in Example 2; "3-1" and "3-2" are both foamed with the pre-foamed particles prepared in Example 3; "4-1" and "4-2" are both foamed with the pre-foamed particles prepared in Example 4; "5-1" and "5-2" are both foamed with the pre-foamed particles prepared in Example 5; "6-1" and "6-2" are both foamed with the pre-foamed particles prepared in Example 6.
[0069] In Table 4 above, in order to clearly indicate the values, the values in the column "molded part surface resistance" are index values. For example, "3" in the column "molded part surface resistance" in 1-1 represents "10 3 ”, and so on.
[0070] Each comparative example of the present invention is compared with Example 3; the differences between each comparative example and Example 3 are as follows:
[0071] The formulas of the conductive masterbatches γ-3, γ-4 and γ-5 in the comparative examples of the present invention are shown in Table 5:
[0072] Table 5
[0073] γ-3 γ-4 γ-5 Polypropylene raw material A (parts by weight) 70 Polypropylene raw material H (parts by weight) 70 Polypropylene raw material I (parts by weight) 70 Conductive carbon black C (parts by weight) 30 30 30
[0074] In the preparation steps of conductive masterbatches γ-3, γ-4 and γ-5, the mixing processing temperature is 170°C; the twin-screw processing temperature is 200°C, the pelletizing size is 30-40mg, the length is 6mm, and the drying temperature is 80°C for 6h.
[0075] The formula of the conductive polypropylene pre-foamed particles in each comparative example is shown in Table 6:
[0076] Table 6
[0077]
[0078] The processing temperature of the core layer is 200°C, the processing temperature of the skin layer is 200°C, the ratio of the extrusion speed of the skin layer to the extrusion speed of the core layer is 1:9, the drawing pellet size is 2 mm long and weighs 1 mg; the polypropylene base material A is a random copolymer polypropylene with a melting point of 150°C and a melt index of 10 (g / 10min / 220°C); the nucleating agent E is zinc borate; the lubricant F is oleic acid amide; the stabilizer G is a mixture of antioxidant 1010 and light stabilizer 622 in a mass ratio of 1:1.
[0079] The pre-foamed particles prepared in the above comparative examples were foamed, and the foaming parameters and performance test data are shown in Table 7:
[0080] Table 7
[0081]
[0082]
[0083] In the above Table 4, "D1-1" and "D1-2" are both foamed with the pre-foamed particles prepared in Comparative Example 1; "D2-1" and "D2-2" are both foamed with the pre-foamed particles prepared in Comparative Example 2; "D3-1" and "D3-2" are both foamed with the pre-foamed particles prepared in Comparative Example 3; "D4-1" and "D4-2" are both foamed with the pre-foamed particles prepared in Comparative Example 4.
[0084] In Table 7, the values in the column “Surface resistance of molded parts” are index values for the sake of clarity. For example, “8” in the column “Surface resistance of molded parts” in D1-1 represents “10 8 ”, and so on.
[0085] Product characterization and performance testing methods are as follows:
[0086] Appearance evaluation of molded parts: visual inspection, including " ★★★★★ "It means the surface is smooth, without defects and has good gloss;" ★★★★☆ "Indicates that there are a few pinholes on the surface;" ☆☆☆★★ "Represents that the appearance of the molded body is average, with many defects on the surface, but it is acceptable under certain conditions;" ☆☆☆☆★ "Indicates that the surface of the product is extremely poor, with many pinholes and low gloss.
[0087] Compression strength: According to GB / T 8813 rigid foam plastic compression strength test.
[0088] Surface resistance of molded parts: For the test method, refer to the national standard "GB / T31838.3-2019" Dielectric and resistance properties of solid insulating materials Part 3: Resistance characteristics (DC method) surface resistance and surface resistivity.
[0089] Absorption performance: tested according to GJB 5239-2004 test method for absorption performance of radio frequency absorbing materials.
[0090] From the above data, it can be seen that the conductive foamed polypropylene beads provided by the present invention have a resistance value covering 10 2-8 It can take into account the characteristics of wave absorption and surface resistance. By adjusting the thickness of the skin, the intensity of wave absorption can be changed. The wave absorption intensity distribution is 40-70db. The appearance of the prepared product is more advantageous than that of conventional conductive products, and the comprehensive performance is better.
[0091] Comparative Example 1 Compared with Example 3, in the preparation process of the conductive masterbatch, the polypropylene raw material A is used to replace the polypropylene base material α. Since the melting point of the polypropylene raw material A is relatively high, the molding temperature is significantly increased, and the prepared conductive foamed polypropylene beads are difficult to burn.
[0092] Compared with Example 3, in Comparative Example 2, during the preparation of the conductive masterbatch, the polypropylene raw material H is used to replace the polypropylene base material α. Since the polypropylene raw material H has a lower melting point, the outer side of the part is easily matured during molding, resulting in poor internal welding and brittle parts. The prepared conductive foamed polypropylene beads cannot be molded and used.
[0093] Comparative Example 3 Compared with Example 3, in the preparation process of the conductive masterbatch, the polypropylene raw material I is used to replace the polypropylene base material α. Since the polypropylene raw material I has a high melting point and is a homopolymer, the melting temperature increases sharply and cannot meet the production needs of downstream customers. The prepared conductive foamed polypropylene beads have poor welding performance, no path can be formed on the surface, and the surface resistance disappears.
[0094] Compared with Example 3, in Comparative Example 4, black masterbatch β is not added to the core layer during the preparation of the conductive masterbatch. Due to the lack of carbon black in the core layer, the product cannot provide wave absorbing properties. The prepared conductive foamed polypropylene beads can only be used for antistatic products but cannot be used for wave absorbing business.
[0095] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A method for preparing conductive foamed polypropylene beads, It is characterized in that The steps include: S1: According to the formula, the polypropylene base material α and the conductive carbon black C are blended in an internal mixer, and then granulated by twin-screw extrusion to obtain a conductive masterbatch γ; The polypropylene base material α has a melting point range of 125°C-130°C and a melt index range of 20-80 (g / 10min / 220°C); S2: Blending polypropylene base material A, dispersant B, conductive carbon black C and carbon black D in an internal mixer, and then extruding and granulating through a twin-screw device to obtain a black masterbatch β; S3: Using a co-extrusion device, the conductive masterbatch γ is used as the skin layer, and the polypropylene base material A, the black masterbatch β, the nucleating agent E, the lubricant F, and the stabilizer G are used as the core layer, and the mixture is blended, drawn, and granulated to obtain conductive polypropylene pre-foamed particles; S4: foaming the conductive polypropylene pre-foamed particles through a supercritical carbon dioxide autoclave pressure foaming process to obtain conductive polypropylene foamed beads.
2. The method for preparing the conductive foamed polypropylene beads according to claim 1, It is characterized in that Step S4 also includes: secondary foaming of the conductive polypropylene foam beads by a steam foaming process.
3. The method for preparing the conductive foamed polypropylene beads according to claim 1, It is characterized in that The preparation method of the polypropylene base material α is as follows: compounding a polypropylene raw material H and a polypropylene raw material I, and adding a dispersant B to obtain a polypropylene base material α; wherein the melting point range of the polypropylene raw material H is 115° C.-125° C.; and the melt index of the polypropylene raw material I is 100-200 (g / 10min / 220° C.).
4. The method for preparing the conductive foamed polypropylene beads according to claim 3, It is characterized in that In the polypropylene base material α, the mass fraction of the polypropylene raw material I is 3%-6%, and the mass fraction of the dispersant B is 2%.
5. A method for preparing conductive foamed polypropylene beads according to any one of claims 1 to 4, It is characterized in that The mass ratio of the polypropylene base material α to the conductive carbon black C in step S1 is (9-7): (1-3).
6. The method for preparing the conductive foamed polypropylene beads according to claim 5, It is characterized in that The particle size of the conductive carbon black C is 200-500 nm.
7. A method for preparing conductive foamed polypropylene beads according to any one of claims 1 to 4, It is characterized in that The polypropylene base material A is random copolymer polypropylene with a melting point of 145-155° C. and a melt index of 5-15 (g / 10min / 220° C.).
8. The method for preparing the conductive foamed polypropylene beads according to claim 7, It is characterized in that The dispersant B is ethylene bisstearamide.
9. The method for preparing the conductive foamed polypropylene beads according to claim 7, It is characterized in that The particle size of the carbon black D is 50-200 nm.
10. The method for preparing the conductive foamed polypropylene beads according to claim 7, It is characterized in that The mass ratio of the polypropylene base material A, the dispersant B, the conductive carbon black C and the carbon black D in step S2 is (35-53): (2-5): (5-10): (40-50).
11. A method for preparing conductive foamed polypropylene beads according to any one of claims 1 to 4, It is characterized in that The mass ratio of the polypropylene base material A, the black masterbatch β, the nucleating agent E, the lubricant F, and the stabilizer G in the core layer of step S3 is (81.7-88.4): (10-15): (0.1-0.3): (1-2): (0.5-1).
12. A conductive foamed polypropylene bead, It is characterized in that The conductive foamed polypropylene beads are prepared by the method for preparing the conductive foamed polypropylene beads according to any one of claims 1 to 11.
13. A molded article, It is characterized in that The conductive foamed polypropylene beads as claimed in claim 12 are obtained by steam molding.