Phthalocyanine-based porous organic polymer aerogel as well as preparation method and application thereof
The preparation of phthalocyanine-based porous organic polymer aerogel by cross-linking reaction of phthalocyanine-based porous polymer with chitosan and polyethyleneimine is solved, and the problem of cumbersome and high cost in the gold recovery process in the prior art is achieved. Efficient and low-cost gold recycling and reuse.
Patent Information
- Application Number
- CN202411168640.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-12
AI Technical Summary
The preparation process of existing porous organic polymer aerogels in gold recycling is cumbersome, with high cost, low selectivity and small adsorption, making it difficult to achieve efficient and highly selective gold recovery.
The phthalocyanine-based porous polymer is prepared by solvothermal reaction and cross-linking with chitosan and polyethyleneimine. The phthalocyanine-based porous polymer is obtained by solvothermal reaction and cross-linking. The phthalocyanine-based porous polymer is obtained by solvothermal reaction and the shell is used. Polysaccharides and polyethyleneimine form crosslinked structures in an acidic environment, improving their chemical chelation and adsorption properties.
It realizes a phthalocyanine-based porous organic polymer aerogel with simple preparation process, low cost, high selectivity and high adsorption capacity. It can efficiently adsorb and reduce gold ions in an acidic environment, and is suitable for gold recycling and reuse.
Smart Images

Figure CN118930955A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of porous organic polymer materials, and in particular to a phthalocyanine-based porous organic polymer aerogel and a preparation method and application thereof. Background Art
[0002] The information disclosed in the background of the invention is only intended to enhance the understanding of the overall background of the invention and should not be necessarily regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] As a precious metal, gold is widely used in jewelry, technology, medicine and other fields. However, the scarcity and irreplaceability of gold have led to its supply shortage. Efficient extraction of gold from secondary resources such as electronic waste can not only make up for the shortage of gold resources, improve resource utilization and economic benefits, but also avoid the serious impact of electronic waste on the ecological environment.
[0004] Porous organic polymers (POPs) are a new type of porous material, which is composed of a variety of organic components bonded by covalent bonds. Some structural units in porous organic polymers can form stable complexes with a variety of metals (especially precious metals), so they are expected to be used in precious metal extraction. However, the insolubility and non-melting properties of porous organic polymers are a major challenge that hinders their practical application. In recent years, the technology of physically mixing porous organic polymer solid powder with a matrix to make bulk materials or membrane materials has become an effective method to improve the practicality of porous organic polymers. However, porous organic polymer particles inevitably fall off from the overall material, causing secondary pollution problems. Another method is to graft a pre-designed porous organic polymer onto a matrix through strong forces such as covalent bonds or hydrogen bonds to construct an overall material, which not only avoids the shedding of porous organic polymer solid powder, but also improves processability and reusability, thereby expanding its practical application range; aerogel, as an ultra-light material with a unique three-dimensional network structure, is a good candidate for substrate material.
[0005] At present, there have been reports on the use of porous organic polymer aerogel materials for gold recovery, but the preparation process is usually cumbersome and costly, which is not conducive to its practical application, or the extraction performance is poor, the selectivity is low, and the adsorption amount is small. Therefore, how to provide a porous organic polymer aerogel material with a simpler preparation process, lower cost, and high efficiency and selectivity for gold recovery is an urgent problem to be solved. Summary of the invention
[0006] In view of this, the present invention provides a phthalocyanine-based porous organic polymer aerogel and a preparation method and application thereof. The phthalocyanine-based porous organic polymer aerogel of the present invention has a simple preparation process and has good elasticity and stability. It also exhibits high adsorption and high selectivity for gold and has broad application prospects.
[0007] In a first aspect, the present invention provides a method for preparing a phthalocyanine-based porous organic polymer aerogel, comprising the following steps:
[0008] Phthalocyanine-based porous polymers were obtained by solvothermal reaction of tetraaminophthalocyanine and 2,5-dihydroxyterephthalaldehyde;
[0009] The phthalocyanine-based porous polymer and chitosan are mixed, and then an acetic acid aqueous solution is added to dissolve by stirring, and then an epichlorohydrin and polyethyleneimine aqueous solution are added, stirred and mixed, and heated to react to obtain a hydrogel;
[0010] The hydrogel is freeze-dried to obtain a phthalocyanine-based porous organic polymer aerogel.
[0011] Preferably, the molar ratio of tetraaminophthalocyanine to 2,5-dihydroxyterephthalaldehyde is 1:(1.8-2.2).
[0012] Preferably, the solvent for the solvothermal reaction is a mixed solvent of o-dichlorobenzene, ethanol and acetic acid aqueous solution, and the volume ratio of o-dichlorobenzene, ethanol and acetic acid aqueous solution is (2-3): (2-3): (0.4-0.6); the concentration of the acetic acid aqueous solution is 4-8 mol / L.
[0013] Preferably, the temperature of the solvothermal reaction is 110-130° C., and the time of the solvothermal reaction is 60-80 hours.
[0014] Preferably, the dosage ratio of the phthalocyanine-based porous polymer, chitosan, acetic acid aqueous solution, epichlorohydrin and polyethyleneimine aqueous solution is (15-25) mg: (30-50) mg: (1-3) mL: (0.1-0.2) mL: (1-3) mL.
[0015] Furthermore, the concentration of the acetic acid aqueous solution is 0.2-0.5 mol / L; the concentration of the polyethyleneimine aqueous solution is 3-5 wt%.
[0016] Preferably, the step of adding acetic acid aqueous solution and stirring and dissolving is carried out under stirring conditions, and the stirring and dissolving time is 20 to 40 minutes; the stirring and mixing time is 20 to 40 minutes.
[0017] Preferably, in the step of obtaining the hydrogel by heating reaction, the temperature of the heating reaction is 50 to 70° C., and the heating reaction time is 3 to 6 hours.
[0018] In a second aspect, the present invention provides a phthalocyanine-based porous organic polymer aerogel prepared by the above preparation method.
[0019] In a third aspect, the present invention provides the use of the above-mentioned phthalocyanine-based porous organic polymer aerogel in gold recovery.
[0020] Compared with the prior art, the present invention has achieved the following beneficial effects:
[0021] (1) The present invention prepares phthalocyanine-based porous organic polymer aerogel by cross-linking reaction and freeze drying, and the preparation method is simple, the conditions are easy to control, and the cost is low;
[0022] (2) The phthalocyanine-based porous organic polymer aerogel prepared by the present invention has strong chemical chelating ability. It has a positive charge property in an acidic environment due to its rich amino group content. It also has good elasticity and stability. It has high absorption capacity and selectivity for gold ions. During the adsorption process, it can reduce gold ions to gold in situ. It can be better applied to the gold recovery process, and can be reused with a long service life, which has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The drawings constituting part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their description are used to explain the present invention and do not constitute an improper limitation of the present invention. Obviously, for those skilled in the art, other drawings can be obtained based on these drawings without creative work.
[0024] Figure 1 is a reaction scheme of step (1) of Example 1 of the present invention;
[0025] Figure 2 It is the infrared spectra of H2TAPc(NH2)4, DHTA and TD-POP and TD-POP@CS / PEI-2 aerogel of Example 1 of the present invention;
[0026] Figure 3 The solid state of TD-POP and TD-POP@CS / PEI-2 aerogel of Example 1 of the present invention is 13 C NMR spectrum;
[0027] Figure 4 is a thermogravimetric analysis diagram of TD-POP@CS / PEI-2 aerogel in Example 1 of the present invention;
[0028] Figure 5 is a scanning electron microscope image of the TD-POP@CS / PEI-2 aerogel of Example 1 of the present invention;
[0029] Figure 6 is the BET specific surface area of TD-POP and TD-POP@CS / PEI-2 of Example 1 of the present invention;
[0030] Figure 7 is a pore size distribution diagram of a non-local density functional theory (NLDFT) model of TD-POP according to Example 1 of the present invention;
[0031] Figure 8 is the adsorption amount and zeta potential diagram of the TD-POP@CS / PEI-2 aerogel of Example 1 of the present invention at different pH values (pH=2-10);
[0032] Fig. 9 is a graph showing the relationship between the adsorption efficiency of gold (III) and time of the TD-POP@CS / PEI-2 aerogel of Example 1 of the present invention;
[0033] Fig.10 is the pseudo-first-order kinetic linear fitting diagram of TD-POP@CS / PEI-2 of Example 1 of the present invention;
[0034] Fig.11 is the pseudo-second-order kinetic linear fitting diagram of TD-POP@CS / PEI-2 of Example 1 of the present invention;
[0035] Fig.12 The figure is the effect of the initial gold concentration of the present invention on the adsorption amount of TD-POP@CS / PEI-2 in Example 1 and the Langmuir and Freundlich isotherm model fitting diagram;
[0036] Fig.13 This is a comparison chart of the adsorption efficiency of TD-POP@CS / PEI-2 of Example 1 of the present invention for different metal ions in a simulated actual leaching solution;
[0037] Fig.14 The Fourier transform infrared spectra of TD-POP@CS / PEI-2 of Example 1 of the present invention after being immersed in 0.1 mol / L HCl and NaOH solution for 3 days are compared with those of the initial TD-POP@CS / PEI-2;
[0038] Fig.15 This is the full XPS spectrum of TD-POP@CS / PEI-2 before and after gold adsorption in Example 1 of the present invention;
[0039] Fig.16 This is the high-resolution Au4fXPS spectrum of TD-POP@CS / PEI-2 after gold adsorption in Example 1 of the present invention;
[0040] Fig.17is a UV-visible-near infrared diffuse reflectance spectrum of the TD-POP of Example 1 of the present invention;
[0041] Fig.18 CV curves of TD-POP@CS / PEI-2 aerogel and ferrocene in Example 1 of the present invention;
[0042] Fig.19 is the Tauc plot of TD-POP@CS / PEI-2 of Example 1 of the present invention;
[0043] Fig. 20 is an energy level diagram of the gold reduction mechanism of Example 1 of the present invention;
[0044] Fig.21 This is a high-resolution XPSN1s spectrum of TD-POP@CS / PEI-2 after gold adsorption in Example 1 of the present invention;
[0045] Fig. 22 This is a test chart of the recycling performance of TD-POP@CS / PEI-2 according to Example 1 of the present invention. DETAILED DESCRIPTION
[0046] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0047] The present invention provides a method for preparing a phthalocyanine-based porous organic polymer aerogel, comprising the following steps:
[0048] Phthalocyanine-based porous polymers were obtained by solvothermal reaction of tetraaminophthalocyanine and 2,5-dihydroxyterephthalaldehyde;
[0049] The phthalocyanine-based porous polymer and chitosan are mixed, and then an acetic acid aqueous solution is added to dissolve by stirring, and then an epichlorohydrin and polyethyleneimine aqueous solution are added, stirred and mixed, and heated to react to obtain a hydrogel;
[0050] The hydrogel is freeze-dried to obtain a phthalocyanine-based porous organic polymer aerogel.
[0051] The present invention first utilizes tetraaminophthalocyanine and 2,5-dihydroxyterephthalaldehyde to undergo Schiff base reaction to obtain a phthalocyanine-based porous polymer (TD-POP), then mixes the obtained phthalocyanine-based porous polymer with chitosan (CS) evenly, then adds an acetic acid solution to promote the dissolution of chitosan, and then adds a dendritic branched polymer polyethyleneimine (PEI) to improve the mechanical properties of the aerogel and give the final aerogel good elasticity, and finally adds epichlorohydrin as a cross-linking agent. TD-POP contains amino groups and hydroxyl groups, CS also contains amino groups and hydroxyl groups, and PEI contains abundant amino groups, which will nucleophilically attack epichlorohydrin to open its ring, thereby forming a network structure aerogel that is cross-linked and covalently bonded. Under acidic conditions, the amino group will be protonated to -NH3 + Thus, the negatively charged AuCl4 - Electrostatic attraction, and the phthalocyanine center and imine bond will react with AuCl4 - A coordination reaction occurs, which enables it to be used for the selective recovery of gold.
[0052] In the present invention, the molar ratio of tetraaminophthalocyanine to 2,5-dihydroxyterephthalaldehyde is 1:(1.8-2.2). One tetraaminophthalocyanine molecule contains four amino groups, and one 2,5-dihydroxyterephthalaldehyde molecule contains two aldehyde groups. The phthalocyanine-based porous polymer is generated by the condensation of the amino groups and the aldehyde groups.
[0053] In the present invention, the solvent for the solvothermal reaction is a mixed solvent of o-dichlorobenzene, ethanol and acetic acid aqueous solution, the volume ratio of o-dichlorobenzene, ethanol and acetic acid aqueous solution is (2-3): (2-3): (0.4-0.6); the concentration of the acetic acid aqueous solution is 4-8 mol / L. The addition of acetic acid can play a certain catalytic role and promote the Schiff base reaction.
[0054] In the present invention, the temperature of the solvothermal reaction is 110-130°C, more preferably 115-125°C; the time of the solvothermal reaction is 60-80h, more preferably 70-80h. The present invention does not impose any special restrictions on the steps of the solvothermal reaction, and the solvothermal reaction method commonly used in the art can be used.
[0055] After the solvent thermal reaction is completed, the present invention further includes the steps of centrifuging, washing and drying the reaction solution. The present invention does not impose any special restrictions on the above-mentioned centrifugation, washing and drying steps, and the commonly used methods in the art can be used.
[0056] In the present invention, the dosage ratio of the phthalocyanine-based porous polymer, chitosan, acetic acid aqueous solution, epichlorohydrin and polyethyleneimine aqueous solution is (15-25) mg: (30-50) mg: (1-3) mL: (0.1-0.2) mL: (1-3) mL. The concentration of the acetic acid aqueous solution is 0.2-0.5 mol / L; the concentration of the polyethyleneimine aqueous solution is 3-5 wt%.
[0057] In the present invention, the step of adding acetic acid aqueous solution and stirring and dissolving is carried out under stirring conditions, and the stirring and dissolving time is 20 to 40 minutes. In the present invention, the stirring and mixing time is 20 to 40 minutes, and the present invention does not impose any special restrictions on the stirring speed.
[0058] In the present invention, in the step of heating reaction to obtain hydrogel, the temperature of the heating reaction is 50-70°C, and the time of the heating reaction is 3-6h. This step of the present invention is preferably carried out in an oven, firstly the mixed solution after stirring and mixing is transferred to a mold, and then the mold is placed in an oven for heating reaction to obtain a hydrogel. The present invention does not impose any special restrictions on the material and size of the mold, and those skilled in the art can customize it according to actual needs.
[0059] The present invention does not impose any particular limitation on the freeze-drying process, and the freeze-drying means commonly used in the art may be used.
[0060] The present invention also provides a phthalocyanine-based porous organic polymer aerogel prepared by the above preparation method. The phthalocyanine-based porous organic polymer aerogel prepared by the present invention has strong chemical chelating ability, has positive charge properties in an acidic environment due to rich amino groups, and has good elasticity and stability.
[0061] The present invention also provides the use of the phthalocyanine-based porous organic polymer aerogel in gold recovery.
[0062] In the present invention, the application includes recovering gold from secondary electronic waste, gold mine wastewater or seawater purification, preferably recovering gold from secondary electronic waste.
[0063] The technical solution of the present invention is further described below in conjunction with specific embodiments. The cylindrical mold in the following embodiments has a specification of 27.5 mm×57 mm (diameter×height) and is made of glass.
[0064] Example 1
[0065] This embodiment provides a method for preparing a phthalocyanine-based porous organic polymer aerogel (TD-POP@CS / PEI-2).
[0066] (1) Synthesis of phthalocyanine-based porous polymer (TD-POP):
[0067] Tetraaminophthalocyanine (H2TAPc(NH2)4, 57.46 mg, 0.2 mmol) and 2,5-dihydroxyterephthalaldehyde (DHTA, 66.45 mg, 0.4 mmol) were added to a polytetrafluoroethylene liner. Then, a solvent (2.5 mL of o-dichlorobenzene, 2.5 mL of anhydrous ethanol, and 0.5 mL of a 6 M aqueous acetic acid solution) was added, and the resulting mixture was ultrasonicated for 10 minutes. Then, the polytetrafluoroethylene liner was placed in a stainless steel hydrothermal reactor and placed in an oven at 120°C for 3 days. After cooling to room temperature, a black solid powder was separated by centrifugation and washed with N,N-dimethylformamide (10 mL×2), acetone (10 mL×2), and tetrahydrofuran (10 mL×2). Finally, the obtained solid was collected and dried in vacuo at 70°C overnight to obtain a black solid powder, recorded as TD-POP (72.16 mg, 74.91%). The reaction scheme of this step is shown in the figure. Figure 1 shown.
[0068] (2) Preparation of phthalocyanine-based porous organic polymer aerogel (TD-POP@CS / PEI-2):
[0069] First, chitosan powder (CS, 40 mg) and TD-POP powder (20 mg) obtained in step (1) were ground in a mortar until uniformly mixed. Then, the mixture was transferred to a small glass bottle, and acetic acid solution (2 mL, 0.35 mol / L) was added and magnetically stirred for 30 minutes. When the mixture became uniform and viscous, epichlorohydrin (155 μL) and 2 mL of 4 wt% polyethyleneimine (PEI) aqueous solution were added and stirred for 30 minutes until a uniform mixture was formed. Then, the mixture was slowly poured into a cylindrical mold and placed in an oven at 60 ° C for 4 hours to obtain a highly cross-linked and stable hydrogel. The hydrogel was placed in a refrigerator for 6 hours and then freeze-dried at -30 ° C for 12 hours to obtain TD-POP@CS / PEI-2 aerogel.
[0070] Test example
[0071] 1. Infrared analysis:
[0072] The chemical composition and molecular structure of H2TAPc(NH2)4, DHTA, TD-POP and TD-POP@CS / PEI-2 aerogels of Example 1 were analyzed by Fourier transform infrared spectroscopy. Figure 2 As shown in the figure, 3212cm -1 The absorption peak nearby belongs to -NH2 of H2TAPc(NH2)4, 1670cm -1The absorption peaks near 1656 cm-1 belong to the C=O stretching vibration of DHTA. In the Fourier transform infrared spectrum of TD-POP, these peaks almost disappeared, while the peak at 1656 cm-1 -1 A peak corresponding to the vibration of the imine bond appeared at 1656 cm -1 Similar vibration peaks also appeared at 1566 cm, which indicates that TD-POP is successfully integrated with the aerogel. In addition, it is worth mentioning that the 1566 cm -1 and 1072cm -1 The characteristic peaks at and belong to CN and COC, respectively, are attributed to the covalent bonds established between TD-POP, CS and PEI under the action of the cross-linking agent epichlorohydrin, which can make the overall material have higher stability.
[0073] 2. Solid State 13 C NMR spectroscopy analysis:
[0074] Solid State 13 C NMR spectroscopy further confirmed the successful synthesis of TD-POP and TD-POP@CS / PEI-2 aerogels in Example 1. Figure 3 As shown in the figure, the peak at 160 ppm belongs to the imine carbon, and the broad peak between 109 and 153 ppm belongs to the phthalocyanine carbon, which indicates that the imine-linked phthalocyanine-based TD-POP was successfully synthesized. In addition, the broad peaks from 38 to 75 ppm in TD-POP@CS / PEI-2 are attributed to CS and PEI. 13 The carbon characteristic signals of TD-POP were observed in the CNMR spectrum, which again proved that TD-POP was successfully integrated into CS / PEI aerogel. In addition, the characteristic peaks at 64 and 80 ppm can be attributed to CN and CO carbons, which again showed that PEI, CS and TD-POP formed covalent bonds under the action of the crosslinker.
[0075] 3. Thermogravimetric analysis (TGA) and morphology analysis:
[0076] Figure 4 Thermogravimetric analysis (TGA) of TD-POP@CS / PEI-2 aerogel of Example 1. Figure 4 It can be seen that when the temperature reaches 120 °C, only a 10% decrease in mass is observed, indicating that it has good thermal stability. Figure 5This is a scanning electron microscope (SEM) image of the TD-POP@CS / PEI-2 aerogel of Example 1, showing a porous and three-dimensional interconnected structure. This structure originates from the cross-linked PEI / CS polymer, which is conducive to the effective mass transfer of guest molecules, thereby significantly improving the subsequent adsorption performance of the aerogel.
[0077] 4. Porosity characterization:
[0078] Porosity is the key to the capture of precious metals, so the BET specific surface area of TD-POP and TD-POP@CS / PEI-2 in Example 1 was calculated based on the N2 adsorption-desorption isotherm data using the BET model, as shown in Figure 6 As shown, the BET surface areas of the two are 28 and 0.17 m 2 / g, and the pore volumes are 0.06635 and 0.01358 cm 3 / g. The pore size distribution diagram of the non-local density functional theory (NLDFT) model is shown in Figure 7 As shown, it shows that the pore size distribution of TD-POP is in the range of 1.71-20.35nm, indicating that TD-POP has mesoporous properties. This characteristic of TD-POP pores provides open and accessible space for precious metal ions, which is conducive to electron transfer, thus providing the possibility of improving adsorption performance.
[0079] 5. Effect of pH value of Au(III) solution on adsorption performance of TD-POP@CS / PEI-2 of Example 1:
[0080] The pH value of the solution may affect the type of ion species and the characteristics of the surface charge of the adsorbent. In order to study the effect of pH on the adsorption of Au(III) by TD-POP@CS / PEI-2 aerogel, adsorption experiments at different pH values (pH = 2-10) and zeta potential tests of TD-POP@CS / PEI-2 aerogel were carried out. The results are shown in Figure 2. Figure 8 As shown. It can be seen that in the pH range of 2 to 5, the adsorption of Au(III) by TD-POP@CS / PEI-2 aerogel increases with the increase of pH value. This may be due to the fact that at low pH values (pH = 2-5), the main form of Au(III) is AuCl4 - The surface potential of TD-POP@CS / PEI-2 aerogels is always positive, which may be due to the -NH2 in PEI and the protonation of the TD-POP edge. Therefore, the negatively charged Au(III) species can be captured by electrostatic interaction with the positively charged TD-POP@CS / PEI-2 aerogels, resulting in excellent adsorption capacity. However, at lower pH values, high concentrations of Cl- will react with AuCl4 -Compete for the positively charged adsorption sites of TD-POP@CS / PEI-2 aerogel. The lower the pH value, the more Cl - AuCl4 - The competition is more intense, resulting in a slight decrease in adsorption capacity. As the pH value increases, AuCl4 - The ions gradually hydrolyze into other ionic forms, such as AuCl3(OH) - 、AuCl2(OH)2 - 、AuCl(OH)3 - and Au(OH)4. Meanwhile, the zeta surface potential of TD-POP@CS / PEI-2 aerogels gradually decreases with increasing pH value in the range of pH 6 to 10. Especially under alkaline conditions, the zeta surface potential drops to negative values, which will lead to electrostatic repulsion between the negatively charged TD-POP@CS / PEI-2 aerogels and Au(III) species.
[0081] 6. Adsorption kinetics of TD-POP@CS / PEI-2 of Example 1:
[0082] Fig. 9 The effect of adsorption time on the adsorption efficiency of gold (III) by TD-POP@CS / PEI-2 aerogel is shown. As can be seen from the figure, the adsorption efficiency increases rapidly in the first half an hour, reaching a maximum of 75%. Subsequently, the adsorption efficiency gradually slows down and stabilizes at around 97% after one hour, indicating that TD-POP@CS / PEI-2 aerogel has a faster adsorption rate and higher adsorption efficiency for gold. Fig.10 ) and pseudo-second-order kinetic model ( Fig.11 ) studied the adsorption kinetics of Au(III) on TD-POP@CS / PEI-2 aerogel. The corresponding data of the two models were analyzed and their correlation coefficient (R 2 ). R of pseudo-first-order model and pseudo-second-order kinetic model 2 The values are 0.9040 and 0.9984, respectively, which obviously means that the latter is considered to be more suitable for describing the adsorption process of Au(III) by TD-POP@CS / PEI-2 aerogel. It is well known that the pseudo-first-order model is based on physical adsorption to control the adsorption process, while the pseudo-second-order kinetic model is based on chemical adsorption to control the adsorption process. Therefore, in the adsorption process of Au(III) by TD-POP@CS / PEI-2 aerogel, chemical adsorption is dominant.
[0083] 7. Adsorption isotherm of TD-POP@CS / PEI-2 of Example 1:
[0084] In order to study the relationship between the adsorption capacity of the TD-POP@CS / PEI-2 aerogel of Example 1 and the initial concentration of Au(III), an adsorption isotherm experiment was performed. Specifically, the aerogel was immersed in Au(III) solutions with initial concentrations ranging from 50 ppm to 750 ppm, and the corresponding equilibrium adsorption amount was calculated. Fig.12 As shown in the figure, the adsorption capacity of the aerogel increases with the increase of the initial Au(III) concentration. When the initial Au(III) concentration is 750ppm, the adsorption amount reaches the maximum value (2088mg / g). Then, the experimental data of equilibrium adsorption capacity and equilibrium concentration were analyzed using the Langmuir and Freundlich isotherm models. It was found that the correlation coefficient of the Langmuir model was 0.9919, which was significantly better than the 0.8364 of the Freundlich model. Subsequently, the theoretical maximum adsorption amount was calculated to be 2190mg / g based on the Langmuir model fitting, which is very close to the experimental result (2088mg / g). Based on the above results, it can be inferred that the adsorption of Au(III) by aerogel is more in line with the Langmuir model, that is, the monolayer adsorption process.
[0085] 8. Adsorption selectivity of TD-POP@CS / PEI-2 of Example 1 for Au(III)
[0086] The actual gold recovery leachate usually contains other metal ions, which may compete with Au(III) ions for adsorption sites, so the selective capture of Au(III) ions by the designed adsorbent is particularly important. In order to study the selectivity of TD-POP@CS / PEI-2 aerogel for Au(III) (concentration of 10 ppm), we prepared a simulated leachate containing interfering metal ions. The interfering metal ions include Cd 2+ 、Co 2+ 、Ni 2+ , Mn 2+ and Cr 6+ (The concentration is 100 ppm each). Fig.13 The adsorption selectivity of TD-POP@CS / PEI-2 aerogel for Au(III) in the presence of multiple interfering metal ions was demonstrated. It can be seen that even if the concentration of interfering ions is 10 times that of the target gold ions, the adsorption selectivity of aerogel for gold is as high as 98.35%. The removal rate of interfering ions is only 4.83%-27.40%, which shows that TD-POP@CS / PEI-2 aerogel has good selectivity for Au(III) ions.
[0087] 9. Stability determination of TD-POP@CS / PEI-2 of Example 1:
[0088] TD-POP@CS / PEI-2 was immersed in 0.1 mol / L HCl and NaOH solutions for 3 days, and then the Fourier transform infrared spectra of the original and immersed materials were measured, as shown in Fig.14 As shown in Figure 2, compared with the initial material, the characteristic peaks of the Fourier transform infrared spectrum of TD-POP@CS / PEI-2 did not change significantly. This shows that the structure of TD-POP@CS / PEI-2 was not destroyed, indicating the stability of its chemical structure.
[0089] 10. Adsorption mechanism of TD-POP@CS / PEI-2:
[0090] In order to further analyze the adsorption mechanism of Au(III) by TD-POP@CS / PEI-2 aerogel in Example 1, we used a series of characterization techniques. First, X-ray photoelectron spectroscopy (XPS) analysis was performed on the original aerogel and the aerogel adsorbed with gold. The results are shown in Figure 2. Fig.15 As shown. The XPS spectra of both aerogels show characteristic peaks belonging to O1s, N1s, C1s and Cl2p. In addition, three new characteristic peaks appeared in the XPS spectrum of gold-adsorbed TD-POP@CS / PEI-2 aerogel, located at 353eV, 336eV and 88eV, belonging to Au 4d3, Au 4d5 and Au 4f, respectively, which undoubtedly confirms the successful adsorption of gold (III) on the aerogel. Further analysis of the high-resolution XPS spectrum of gold 4f revealed that it can be divided into six peaks ( Fig.16 ). Among them, 87.92eV (Au 4f 5 / 2 ) and 84.24 eV (Au 4f 7 / 2 ) belongs to Au(0), 88.77eV(Au 4f 5 / 2 ) and 84.79 eV (Au 4f 7 / 2 ) belongs to Au(I), 91.08eV(Au 4f 5 / 2 ) and 87.20 eV (Au 4f 7 / 2 ) are from Au(III). These results indicate that the gold(III) adsorbed on the TD-POP@CS / PEI-2 aerogel is partially reduced to gold(I) and gold(0). As we all know, phthalocyanine and its derivatives are a class of classic photosensitizers with strong near-infrared absorption efficiency. When phthalocyanine is integrated into polymer materials, the light utilization efficiency of the material will be further improved due to the extended π-conjugated framework of TD-POP, which is also confirmed by its UV-visible-near-infrared diffuse reflectance spectrum ( Fig.17 ). Therefore, TD-POP@CS / PEI-2 aerogel has the potential to induce gold reduction:
[0091] AuCl4 - +3e- →Au(s)+4Cl - (aq)+1.002V.
[0092] In order to explore the reduction mechanism, the CV curve ( Fig.18 ) and Tauc curve ( Fig.19 ) determined the energy level of TD-POP@CS / PEI-2 aerogel. The lowest unoccupied molecular orbital (LUMO) of the aerogel was calculated to be about -3.61eV. Using the LUMO potential and the 2.15eV band gap obtained by the Tauc curve, the highest occupied molecular orbital (HOMO) potential of the aerogel can be calculated to be -5.76eV. Fig. 20 As shown, it can be observed that AuCl4 - The standard reduction potential of Au(0) (E0 = 1.002 V vs NHE) is between the HOMO and LUMO of TD-POP@CS / PEI-2 aerogel, indicating that the excited electrons of TD-POP@CS / PEI-2 aerogel can be effectively transferred to Au(III), thereby promoting the reduction of Au(III).
[0093] In addition to the reduction mechanism, it can be seen that the phthalocyanine-N peak (397.70 eV) and imine-N peak (398.45 eV) in the high-resolution XPS spectrum shift to higher binding energies of 399.75 eV and 399.21 eV after adsorption ( Fig.21 ), indicating that there is a strong coordination interaction between the phthalocyanine-N and imine-N functional groups and the gold species. In addition, the amino-N peak of the gold-adsorbed TD-POP@CS / PEI-2 aerogel shifted from 400.10 eV to a higher binding energy of 401.55 eV due to protonation. This indicates that the negatively charged AuCl4 - It can be adsorbed by aerogel through electrostatic action. According to the above experimental results, it can be inferred that the adsorption mechanism of gold (III) by TD-POP@CS / PEI-2 aerogel can be attributed to the interaction between cationic aerogel and AuCl4 - The electrostatic interaction between anions, the strong coordination between N active sites and gold (III), and the reduction effect of TD-POP@CS / PEI-2 aerogel on gold (III) were investigated.
[0094] Application Examples
[0095] This application example provides a recycling performance of the phthalocyanine-based porous organic polymer (TD-POP@CS / PEI-2) aerogel of Example 1.
[0096] 10 mg of TD-POP@CS / PEI-2 aerogel was immersed in 20 mL of 500 mg / L gold (III) solution. After adsorption for 24 h, the gold-adsorbed TD-POP@CS / PEI-2 was desorbed with thiourea solution (containing 10 wt% thiourea and 5 wt% hydrochloric acid) and put into the next cycle, and was recycled for a total of 8 times. Fig. 22 The results of the aerogel cycle test are shown. It can be seen that in the first four cycles, the recovery rate of gold can reach more than 90%. In the next four cycles, the recovery rate gradually decreased, but it still exceeded 80%, indicating that the reuse performance of TD-POP@CS / PEI-2 is excellent.
[0097] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a phthalocyanine-based porous organic polymer aerogel, characterized in that: The steps include: Phthalocyanine-based porous polymers were obtained by solvothermal reaction of tetraaminophthalocyanine and 2,5-dihydroxyterephthalaldehyde; The phthalocyanine-based porous polymer and chitosan are mixed, and then an acetic acid aqueous solution is added to dissolve by stirring, and then an epichlorohydrin and polyethyleneimine aqueous solution are added, stirred and mixed, and heated to react to obtain a hydrogel; The hydrogel is freeze-dried to obtain a phthalocyanine-based porous organic polymer aerogel.
2. The preparation method according to claim 1, characterized in that The molar ratio of the tetraaminophthalocyanine to 2,5-dihydroxyterephthalaldehyde is 1:(1.8-2.2).
3. The preparation method according to claim 1, characterized in that: The solvent for the solvothermal reaction is a mixed solvent of o-dichlorobenzene, ethanol and acetic acid aqueous solution, and the volume ratio of o-dichlorobenzene, ethanol and acetic acid aqueous solution is (2-3): (2-3): (0.4-0.6); the concentration of the acetic acid aqueous solution is 4-8 mol / L.
4. The preparation method according to claim 1, characterized in that: The temperature of the solvent thermal reaction is 110-130° C., and the time of the solvent thermal reaction is 60-80 hours.
5. The preparation method according to claim 1, characterized in that: The dosage ratio of the phthalocyanine-based porous polymer, chitosan, acetic acid aqueous solution, epichlorohydrin and polyethyleneimine aqueous solution is (15-25) mg: (30-50) mg: (1-3) mL: (0.1-0.2) mL: (1-3) mL.
6. The preparation method according to claim 5, characterized in that: The concentration of the acetic acid aqueous solution is 0.2-0.5 mol / L; the concentration of the polyethyleneimine aqueous solution is 3-5 wt %.
7. The preparation method according to claim 1, characterized in that: The step of adding acetic acid aqueous solution and stirring and dissolving is carried out under stirring conditions, and the stirring and dissolving time is 20 to 40 minutes; the stirring and mixing time is 20 to 40 minutes.
8. The preparation method according to claim 1, characterized in that: In the step of obtaining the hydrogel by heating reaction, the temperature of the heating reaction is 50 to 70° C., and the time of the heating reaction is 3 to 6 hours.
9. The phthalocyanine-based porous organic polymer aerogel prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the phthalocyanine-based porous organic polymer aerogel as claimed in claim 9 in gold recovery.