Heat-conducting filler as well as preparation method and application thereof
By grinding the α-alumina powder with organic solvents and coupling agent in thermally conductive silicone, forming an active interface and bonding, the problems of low thermal conductivity and large addition amount are solved, high thermal conductivity and uniform dispersion are achieved, and the Thermal dissipation effect of lithium battery thermally conductive silicone film.
Patent Information
- Application Number
- CN202411016118.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-27
- Publication Date
- 2024-11-12
AI Technical Summary
When modified alumina is used alone as thermal filler in existing thermal conductivity silicones, the thermal conductivity is low and needs to be added in large quantities, which affects other properties such as flexibility and elasticity.
By grinding the α-alumina powder with organic solvent and coupling agent at 60-85°C, an active interface is formed and bonded, a thermal filler with high thermal conductivity is prepared, reducing the amount of addition and improving the thermal conductivity effect.
The prepared thermal conductivity filler can achieve a higher thermal conductivity when used, and the formed cladding layer makes it more uniformly dispersed in the matrix material, avoiding break-out partitions, improving the thermal conductivity and reducing the amount of addition.
Smart Images

Figure BDA0004965715910000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of insulating heat-conducting materials, and in particular relates to a heat-conducting filler and a preparation method and application thereof. Background Art
[0002] Insulating thermally conductive materials are widely used in the automotive, electronic and new energy fields, especially in the lithium battery field. For example, in lithium batteries, the battery pack takes away the heat generated by charging and discharging through heat exchange with the cooling tube, but the direct contact surface between the battery pack and the cooling tube is too small, which affects the heat dissipation effect. Therefore, using thermally conductive silicone sheets to fill the gap between the battery and the cooling tube is an effective way to improve the thermal conductivity. The thermal conductivity of the thermally conductive silicone sheet is crucial to the thermal conductivity effect. Thermally conductive silicone is usually composed of silicone rubber and thermally conductive particles as thermally conductive fillers. Alumina has the advantages of thermal conductivity, insulation, and stable performance. It is used as a thermally conductive filler in thermally conductive silicone.
[0003] Chinese patent CN117247765A discloses a thermally conductive silicone glue and a silicone pad with high thermal conductivity. When a thermally conductive filler composed of modified alumina and modified silicon nitride is added to the thermally conductive silicone glue to improve the thermal conductivity of the thermally conductive silicone pad, or when modified silicon nitride is used alone as a thermally conductive filler, the thermal conductivity effect is better; but when modified alumina is used alone in Example 1, the thermal conductivity of the obtained product is only 5W / m·K., and at this time the amount of modified alumina used is large, 2000 parts by weight, accounting for 95.2% of the total weight of the raw materials. Such a large amount of thermally conductive fillers used to improve thermal conductivity will affect other properties of the silicone pad, such as flexibility and elasticity. Summary of the invention
[0004] The purpose of the present invention is to provide a thermally conductive filler with high thermal conductivity, which can reduce the amount of addition during use and achieve a better thermal conductive effect.
[0005] The technical solution of the present invention is:
[0006] A method for preparing a thermally conductive filler comprises the following steps:
[0007] Step 1: Grind α-alumina powder, organic solvent and coupling agent at 60-85°C for 2-10 hours until the alumina powder D 50 Less than 5μm;
[0008] Step 2, drying to make its moisture content ≤ 0.5% to obtain a thermal conductive filler;
[0009] Wherein: the coupling agent is a stearic acid coupling agent, a silane coupling agent or a titanate coupling agent, and the amount of the coupling agent is 0.4-0.8% by weight of α-alumina; the organic solvent is at least one of methanol, ethanol, acetone and furan, and the amount of the coupling agent is 10-30% by weight.
[0010] As the silane coupling agent, vinyltriethoxysilane, γ-aminopropyltriethoxysilane, 3-mercaptopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, and the like can be used.
[0011] As the titanate coupling agent, triisostearoyl titanate, isopropyl triisostearoyl titanate, isopropoxy tri(dioctyl pyrophosphate) titanate, and the like can be used.
[0012] The preparation method of the thermal conductive filler of the present invention comprises the following steps: adding an organic solvent and a coupling agent to an α-alumina powder, and grinding the mixture under the condition of 60-85°C. On the one hand, the organic solvent disperses the coupling agent so that the coupling agent is uniformly mixed with the α-alumina powder; on the other hand, the organic solvent acts as a grinding medium to lubricate the α-alumina powder and the coupling agent, so that the α-alumina powder particles can roll and slide at multiple angles during the grinding process, thereby causing the α-alumina powder to be continuously squeezed, worn and broken at multiple angles, and continuously exposing more new active interfaces and active sites. During the grinding process, under the condition of 60-85°C, the new active interfaces and active sites continuously exposed on the surface of the α-alumina powder contact with the coupling agent and are squeezed and bonded to each other to form a strong chemical bond. In the thermal conductive filler thus prepared, the alumina on the surface of the ground alumina powder is bonded with the coupling agent and modified, so that the surface of the alumina is activated, and the activation effect is more stable. After drying in step 2, the excess organic solvent and the moisture absorbed during the grinding process are removed, and an active thermal conductive filler aluminum oxide is obtained, which has good thermal conductivity.
[0013] In the above method of the present invention, grinding is carried out at a temperature of 60-85°C, and the coupling agent and the alumina powder are first mechanically mixed and then bonded, so that a coating layer tightly bonded to the alumina is formed on the surface of the dried alumina. In the grinding process, temperature is very important for bonding. Too low or too high a temperature will affect the bonding effect, resulting in poor bonding between the coating layer and the alumina, so that the thermal conductivity of the thermal conductive filler is low when used. The thermal conductive filler prepared by the method of the present invention forms a coating layer formed by bonding the coupling agent and the alumina on the surface of the alumina. The coating layer makes it easier to disperse the alumina in the matrix material when used as a thermal conductive filler, and the distribution in the matrix material is more uniform, so that the product does not produce a short circuit-like partition when conducting heat, and the thermal conductivity of the product is high, thereby achieving a good thermal conductive effect with a small amount of thermal conductive filler. The drying in step 2 can make the water content of the alumina below 0.5% while removing the organic solvent, so as to avoid the formation of a partitioning void when the thermal conductive filler is used. Increase the thermal resistance.
[0014] Preferably, D of α-alumina before grinding 50The particle size before grinding is too large, which will reduce the grinding efficiency and prolong the grinding time. If the grinding time is too long, the organic solvent will be lost, the quality of the grinding product will be difficult to control, the lubrication degree will be insufficient, the grinding will be uneven, and the aluminum oxide will stick and agglomerate during grinding, which will affect the exposure of the active interface and active sites and their bonding with the coupling agent. Of course, organic solvents can be added at the appropriate time to make up for it.
[0015] Preferably, the moisture content of α-alumina before grinding is not more than 0.5%. The moisture content of α-alumina itself is not high, but it is not advisable to mix too much water into it before grinding, especially not to add too much water during the grinding process. Excessive moisture will affect the bonding between the coupling agent and α-alumina, thereby affecting the thermal conductivity of the manufactured thermal conductive filler during use.
[0016] Preferably, the coupling agent contains an organic weak acid aqueous solution with a mass concentration of 10-20%, the volume of the organic weak acid aqueous solution is 25-55% of the total volume of the organic solvent and the organic weak acid aqueous solution, and the organic weak acid is at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.
[0017] When adding organic weak acid solution to the coupling agent, the hydrogen ions ionized by the organic weak acid combine with a small amount of hydroxide on the surface of alumina during the grinding process, which makes the alumina particles with a small amount of charge on the surface. On the one hand, the small amount of charge makes the alumina particles repel each other, increases the stability of the alumina surface, and prevents the mutual agglomeration of alumina particles; promotes the dispersion of alumina in the solvent, and helps the contact and reaction between alumina and the coupling agent; on the other hand, it enhances the surface activity of alumina, which is conducive to the bonding between alumina and the coupling agent, so that alumina and the coupling agent are more and more firmly bonded, further improving the thermal conductivity of the thermal conductive filler in use.
[0018] The present invention also provides a thermally conductive filler, which is made by the above preparation method.
[0019] The thermally conductive filler prepared by the present invention allows the surface of the α-alumina powder to continuously generate new active interfaces and active sites during the grinding process to chemically bond with the coupling agent, thereby improving the thermal conductivity of the prepared thermally conductive filler when in use. When in use, the amount added can be reduced to achieve a better thermal conductive effect.
[0020] The present invention also provides an application of the thermally conductive filler, which is applied to thermally conductive silicone products; the weight percentage of the thermally conductive filler is 30-80%.
[0021] When the heat-conductive filler of the present invention is applied to heat-conductive silicone products, the added amount is small and the heat-conductive effect is good.
[0022] Preferably, the thermally conductive silicone product is a thermally conductive silicone sheet for lithium batteries, and the weight of the thermally conductive filler in the thermally conductive silicone sheet for lithium batteries accounts for 50%-70%. The thermally conductive silicone sheet for lithium batteries obtained by the present invention has good thermal conductivity, can improve the heat dissipation effect, effectively reduce the temperature of lithium batteries, reduce heat accumulation, and extend the life of the battery.
[0023] Preferably, the preparation of the thermally conductive silicone sheet for lithium batteries comprises the following steps: uniformly mixing the silicone rubber substrate and the thermally conductive filler, then adding polymethylphenylsiloxane and octyl polymethylsiloxane and stirring evenly, extruding and drying. Preferably, the silicone rubber substrate is vinyl silicone oil. The vinyl silicone oil is selected from double-end vinyl silicone oil, single-end vinyl silicone oil, side vinyl silicone oil and end-side vinyl silicone oil, and the vinyl content of the vinyl silicone oil is 0.1-2%.
[0024] After the heat-conducting filler is uniformly mixed with the silicone rubber substrate, a cross-linking reaction is carried out with polymethylphenylsiloxane and octyl polymethylsiloxane to form a three-dimensional network structure, so that the heat-conducting filler of the present invention is uniformly dispersed in the cross-linking structure of the silicone product, so that the heat conduction of the silicone product is more uniform, the thermal resistance is smaller, and the thermal conductivity coefficient is larger. And the silicone product made in this way is not easy to deform or break during use. Octyl polymethylsiloxane can form a layer of organic silicon film on the surface of the silicone product, and the organic silicon film can also improve the interface adhesion of the heat dissipation gasket, improve the surface properties of the heat dissipation gasket, and increase its heat resistance, weather resistance and chemical resistance. At the same time, octyl polymethylsiloxane has good antioxidant properties, which can effectively prevent the oxidation and aging of the heat dissipation gasket in a high temperature environment, help to extend the service life of the heat dissipation gasket, and maintain good heat dissipation performance; and octyl polymethylsiloxane has good wettability, which can make the heat dissipation gasket better fit the battery surface, reduce contact resistance, and improve the heat transfer efficiency.
[0025] The beneficial effects of the present invention are:
[0026] The preparation method of the thermal conductive filler of the present invention comprises the following steps: adding an organic solvent and a coupling agent to α-alumina powder and grinding the powder at 60-85° C. The grinding allows the coupling agent to bond with the continuously generated active interface of alumina to form a strong chemical bond, thereby preparing a thermal conductive filler with good active thermal conductivity. When the thermal conductive filler prepared by the present invention is applied to thermal conductive silicone products, the amount used is small and the thermal conductive effect is good. DETAILED DESCRIPTION
[0027] The present invention is described in detail below with reference to the embodiments.
[0028] Example 1
[0029] 1. Prepare a thermally conductive filler as follows:
[0030] Step 1: D50 α-alumina powder with a diameter of 70 μm and a water content of 0.5%, anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane were mixed in a weight ratio of 1:0.0012:0.006 and ground in a continuous ball mill at 70°C for 6 hours until the D of the alumina powder was 50 4.9μm;
[0031] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0032] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0033] The thermal conductive filler prepared in the present embodiment and vinyl silicone oil-terminated vinyl polydimethylsiloxane (vinyl content of 0.13%) were mixed evenly to obtain a base material, and then polymethylphenylsiloxane and octyl polymethylsiloxane were added and stirred evenly, extruded, and then dried to obtain a lithium battery thermal conductive silicone sheet with a thickness of about 2 mm. The weight ratio of the thermal conductive filler, vinyl silicone oil, polymethylphenylsiloxane and octyl polymethylsiloxane was 45:30:7.5:3.5.
[0034] Example 2
[0035] 1. Prepare a thermally conductive filler as follows:
[0036] Step 1:
[0037] Take 0.0012 parts by weight of methanol;
[0038] Preparation of acidified stearic acid coupling agent: Take 15% oxalic acid aqueous solution, the volume of which is the same as the volume of the above 0.0012 parts by weight of methanol, and add it to 0.008 parts by weight of stearic acid coupling agent to obtain acidified stearic acid coupling agent.
[0039] Then pour 0.0012 parts by weight of methanol into the above acidified stearic acid coupling agent, mix well, and pour 1 part by weight of D 50 The mixture was mixed with α-alumina powder with a diameter of 70 μm and a moisture content of 0.5%, and ground in a continuous ball mill at 70°C for 6 hours until the D 50 4.0μm;
[0040] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0041] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0042] The thermally conductive filler prepared in this embodiment is used to prepare a thermally conductive silicone sheet for lithium batteries using the same method as in Example 1, except that the weight ratio of the thermally conductive filler, vinyl silicone oil, polymethylphenylsiloxane and octyl polymethylsiloxane in this embodiment is 90:30:7.5:3.5.
[0043] Example 3
[0044] 1. Prepare a thermally conductive filler as follows:
[0045] Step 1:
[0046] Take 0.0024 parts by weight of acetone;
[0047] Preparation of acidified titanate coupling agent: Take a propionic acid aqueous solution with a mass concentration of 20%, the volume of which is 1 / 3 of the volume of the above 0.0024 parts by weight of acetone, and add it to 0.008 parts by weight of titanate coupling agent triisostearyl titanate to obtain an acidified titanate coupling agent.
[0048] Then pour 0.0024 parts by weight of acetone measured above into the acidified titanate coupling agent, mix well, and pour 1 part by weight of D 50 The mixture was mixed with α-alumina powder with a diameter of 60 μm and a water content of 0.2%, and ground in a continuous ball mill at 60°C for 2 hours until the D 50 3.0μm;
[0049] Step 2: drying to make the moisture content of the mixture 0.2% to obtain a thermally conductive filler.
[0050] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0051] The same method as in Example 1 was used for preparation.
[0052] Example 4
[0053] 1. Prepare a thermally conductive filler as follows:
[0054] Step 1:
[0055] Take 0.0014 parts by weight of furan;
[0056] Preparation of acidified stearic acid coupling agent: Take a 15% formic acid aqueous solution, the volume of which is 1.2 times the volume of the above 0.0014 parts by weight of furan, and add it to 0.007 parts by weight of stearic acid coupling agent to obtain an acidified stearic acid coupling agent.
[0057] Then pour 0.0014 parts by weight of furan measured above into the obtained acidified stearic acid coupling agent, mix well, pour 1 part by weight of D 50The mixture was mixed with α-alumina powder with a diameter of 90 μm and a water content of 0.2%, and ground in a continuous ball mill at 70°C for 10 hours until the D 50 The particle size was 4.9 μm. After grinding for 6 hours, an appropriate amount of furan was added.
[0058] Step 2: drying to make the moisture content of the mixture 0.2% to obtain a thermally conductive filler.
[0059] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0060] The same method as in Example 1 was used for preparation.
[0061] Example 5
[0062] 1. Prepare a thermally conductive filler as follows:
[0063] Step 1:
[0064] Take 0.0004 parts by weight of anhydrous ethanol;
[0065] Preparation of acidified silane coupling agent: Take 10% acetic acid aqueous solution, the volume of which is the same as the volume of the above 0.0004 parts by weight of anhydrous ethanol, and add it to 0.004 parts by weight of silane coupling agent vinyltriethoxysilane to obtain an acidified silane coupling agent.
[0066] Then pour 0.0004 parts by weight of anhydrous ethanol into the obtained acidified silane coupling agent and mix well; pour 1 part by weight of D 50 The mixture was ground in a continuous ball mill at 85°C for 10 hours until the D 50 4.0μm;
[0067] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0068] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0069] The same method as in Example 1 was used for preparation.
[0070] Example 6
[0071] 1. Prepare a thermally conductive filler as follows:
[0072] Step 1:
[0073] Take 0.0020 parts by weight of anhydrous ethanol;
[0074] Preparation of acidified stearic acid coupling agent: Take a 15% citric acid aqueous solution, the volume of which is the same as the volume of the above 0.0020 parts by weight of anhydrous ethanol, and add it to 0.008 parts by weight of stearic acid coupling agent to obtain an acidified stearic acid coupling agent.
[0075] Then pour 0.0020 parts by weight of anhydrous ethanol into the obtained acidified stearic acid coupling agent, mix well, and pour 1 part by weight of D 50 The mixture was mixed with α-alumina powder with a diameter of 70 μm and a moisture content of 0.5%, and ground in a continuous ball mill at 80°C for 6 hours until the D 50 4.0μm;
[0076] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0077] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0078] The same method as in Example 1 was used for preparation.
[0079] Example 7
[0080] 1. Prepare a thermally conductive filler as follows:
[0081] Step 1:
[0082] Take 0.0020 parts by weight of anhydrous ethanol;
[0083] Preparation of acidified stearic acid coupling agent: Take a 15% fumaric acid aqueous solution, the volume of which is the same as the volume of the above 0.0020 parts by weight of anhydrous ethanol, and add it to 0.008 parts by weight of stearic acid coupling agent to obtain an acidified stearic acid coupling agent.
[0084] Then pour 0.0020 parts by weight of anhydrous ethanol into the acidified stearic acid coupling agent obtained above, mix well, and pour 1 part by weight of D 50 The mixture was mixed with α-alumina powder with a diameter of 70 μm and a moisture content of 0.5%, and ground in a continuous ball mill at 80°C for 6 hours until the D 50 4.0μm;
[0085] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0086] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0087] The thermally conductive filler prepared in this embodiment is used to prepare a thermally conductive silicone sheet for lithium batteries using the same method as in Example 1, except that the weight ratio of the thermally conductive filler, vinyl silicone oil, polymethylphenylsiloxane and octyl polymethylsiloxane in this embodiment is 20:30:7.5:3.5.
[0088] Comparative Example 1
[0089] 1. Prepare a thermally conductive filler as follows:
[0090] Step 1: D 50 α-alumina powder with a particle size of 4.9 μm and a moisture content of 0.5% and γ-glycidyloxypropyltrimethoxysilane are mixed in a weight ratio of 1:0.006, and then anhydrous ethanol is added in an amount that all materials become a flowable slurry, and stirred continuously at 70°C in a paddle stirring container for 6 hours.
[0091] Step 2: drying to make the moisture content of the mixture 0.5% to obtain a thermally conductive filler.
[0092] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0093] The same method as in Example 1 was used for preparation.
[0094] Comparative Example 2
[0095] 1. Prepare a thermally conductive filler as follows:
[0096] Step 1: adding anhydrous ethanol and deionized water in a paddle stirring container at a volume ratio of 1:10 to obtain a mixed solvent, and adjusting the pH value of the mixed solvent to 4; adding D 50 α-alumina powder of 4.9 μm is added until the material becomes a flowable slurry. Then γ-glycidyloxypropyltrimethoxysilane is added as a silane coupling agent, and the added mass of the silane coupling agent is 0.6% of the alumina; the temperature is raised to 25°C, and stirred at 30 rpm for 30 minutes; filtered and dried to remove the mixed solvent, and the water content is 0.5% to obtain a thermal conductive filler.
[0097] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0098] The same method as in Example 1 was used for preparation.
[0099] Comparative Example 3
[0100] 1. Preparation of a thermally conductive filler. The difference between the preparation method of this comparative example and that of Example 1 is that the drying in step 2 of this comparative example is only air-dried to remove anhydrous ethanol. The moisture content is measured to be 0.8%, which may be due to water absorption during the production process.
[0101] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0102] The same method as in Example 1 was used for preparation.
[0103] Comparative Example 4
[0104] 1. Preparation of a thermally conductive filler
[0105] Direct use moisture content is 4.9%, D 50 5 μm α-alumina powder is a thermally conductive filler.
[0106] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0107] The same method as in Example 1 was used for preparation.
[0108] Comparative Example 5
[0109] 1. Preparation of a thermally conductive filler
[0110] The only difference between the preparation methods of this comparative example and Example 1 is that the temperature of grinding for 6 hours in the continuous ball mill in step 1 of this comparative example is 50°C.
[0111] 2. Preparation of thermal conductive silicone sheet for lithium battery
[0112] The same method as in Example 1 was used for preparation.
[0113] Performance Testing:
[0114] 1. Testing the activation index of the thermally conductive filler
[0115] The activation index of the thermally conductive fillers prepared in the above embodiments and comparative examples was tested respectively according to the following method. The test results are shown in Table 1.
[0116] Test method: Take 5.000g of thermal conductive filler in a separatory funnel, add 200mL of distilled water, and shake it back and forth at a speed of 120 times / min for 1min. Gently place it on the funnel stand and let it stand for 20min. When it is clearly stratified, take the sample on the water surface, filter out the sinking sample, dry it at 105℃±2℃ until the mass is constant, weigh it, and calculate the mass fraction of the sample on the water surface, which is the activation index.
[0117] 2. Test the thermal conductivity of the prepared lithium battery thermal conductive silicone sheet
[0118] The thermal conductivity of the lithium battery thermal conductive silicone sheets prepared in the above embodiments and comparative examples was tested using the ASTM D5470 standard. The test results are shown in Table 1.
[0119] Table 1
[0120]
[0121] From the data in Table 1, it can be seen that the thermal conductive filler prepared by the method of the present invention has a high activation index. When the amount of the thermal conductive filler added is 52.3% by mass, the thermal conductivity of the lithium battery thermal conductive silicone sheet prepared by the method is 2.09-2.45 W / m·k, which has good thermal conductivity. In addition, in Examples 2-7 where an appropriate amount of organic weak acid is added to the coupling agent, the activation index of the thermal conductive filler is further improved, and the thermal conductivity is even better.
[0122] It can also be seen from Table 1 that:
[0123] Comparative Example 1: No grinding was performed and D 50 α-alumina powder with a diameter of 4.9 μm and a water content of 0.5% was mixed with anhydrous ethanol and γ-glycidyloxypropyltrimethoxysilane. Although the other conditions were exactly the same as those in Example 1, the activation index of the obtained thermal conductive filler was only 79.2%; the thermal conductive silicone sheet for lithium batteries prepared by the same proportion and method as in Example 1 also had significantly poor thermal conductivity, with a thermal conductivity coefficient of only 1.55 W / m·k. It can be seen that grinding plays a key role in the bonding between the coupling agent and the α-alumina powder.
[0124] Comparative Example 2 was not ground and D 50 The α-alumina powder with a diameter of 4.9 μm was added with anhydrous ethanol and deionized water, stirred to react with γ-glycidyloxypropyltrimethoxysilane, and the activation index of the obtained thermal conductive filler was only 79.3%; the thermal conductive silicone sheet for lithium batteries prepared by the same proportion and method as in Example 1 also had significantly poor thermal conductivity, with a thermal conductivity coefficient of 1.56 W / m·k. The method used in the comparative example is similar to the method of Chinese patent CN117247765A, which does not perform grinding, and there is more water in the reaction, which results in the reaction between the coupling agent and the α-alumina powder being hindered, and basically only physical mixing is performed without sufficient chemical bonding, and the thermal conductivity of the α-alumina powder is not significantly improved.
[0125] Although the difference between Comparative Example 3 and Example 1 is only that the drying in step 2 is incomplete, so that the moisture content of the thermally conductive filler reaches 0.8%, and the activation index of the obtained thermally conductive filler does not deteriorate much, the thermal conductivity of the lithium battery thermally conductive silicone sheet prepared therefrom deteriorates a lot. This is because the thermally conductive filler absorbs water during the preparation process and is mixed between the thermally conductive filler powders. When the lithium battery thermally conductive silicone sheet is made, this water cannot be removed, and the inclusion of water forms bubbles, which increases the thermal resistance and deteriorates the thermal conductivity.
[0126] For Comparative Example 4, which used α-alumina powder as a thermal conductive filler without any treatment, the activation index of the α-alumina powder used in Example 1 was very low, only 70.0%, and the thermal conductivity of the lithium battery thermal conductive silicone sheet prepared therefrom was very poor, with a thermal conductivity coefficient of 1.15 W / m·k. It can be seen that directly using α-alumina powder cannot meet the thermal conductivity and heat dissipation requirements of lithium batteries.
[0127] The activation index of the thermal conductive filler in Comparative Example 5 is also relatively low, only 78.5%. The only difference between Comparative Example 5 and Example 1 is that the temperature of grinding in the continuous ball mill for 6 hours in step 1 is 50°C, which does not reach 60-85°C of the present invention. It can be seen that maintaining a suitable reaction temperature is a necessary condition for the reaction of α-alumina powder and coupling agent during grinding.
[0128] The method of the present invention comprises grinding α-alumina powder, an organic solvent and a coupling agent at 60-85° C. for 2-10 hours until the alumina powder D 50 The particle size of the thermal conductive filler is less than 5 μm; and then the thermal conductive filler is dried to a moisture content of ≤0.5% to obtain a thermal conductive filler having a good activation index. When the thermal conductive silicone sheet for lithium batteries is made, the amount used is small and the thermal conductive performance is good.
[0129] It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in the various embodiments of the present invention described above can be combined with each other as long as they do not conflict with each other. In addition, the above are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work belong to the scope of protection of the present invention.
Claims
1. A method for preparing a thermally conductive filler, characterized in that: The following steps are involved: Step 1: Grind α-alumina powder, organic solvent and coupling agent at 60-85°C for 2-10 hours until the alumina powder D 50 Less than 5μm; Step 2, drying to make its moisture content ≤ 0.5% to obtain a thermal conductive filler; Wherein: the coupling agent is a stearic acid coupling agent, a silane coupling agent or a titanate coupling agent, and the amount of the coupling agent is 0.4-0.8% by weight of α-alumina; the organic solvent is at least one of methanol, ethanol, acetone and furan, and the amount of the coupling agent is 10-30% by weight.
2. The method for preparing the thermally conductive filler according to claim 1, characterized in that: D of α-alumina before grinding 50 60-80μm.
3. The method for preparing the thermally conductive filler according to claim 1, characterized in that: The moisture content of α-alumina before grinding is not more than 0.5%.
4. The method for preparing the thermally conductive filler according to claim 1, characterized in that: The coupling agent contains an organic weak acid aqueous solution with a mass concentration of 10-20%, the volume of the organic weak acid aqueous solution is 25-55% of the total volume of the organic solvent and the organic weak acid aqueous solution, and the organic weak acid is at least one of formic acid, acetic acid, propionic acid, oxalic acid and citric acid.
5. A thermally conductive filler, characterized in that: Prepared by the preparation method of any one of claims 1 to 4.
6. The use of the thermally conductive filler as claimed in claim 5, characterized in that: Applicable to thermally conductive silicone products; the thermally conductive silicone products contain the thermally conductive filler described in claim 5.
7. The use of the thermally conductive filler as claimed in claim 6, characterized in that: The weight percentage of the thermal conductive filler is 30-80%.
8. The use of the thermally conductive filler as claimed in claim 6, characterized in that: The thermally conductive silicone product is a thermally conductive silicone sheet for lithium batteries, and the weight of the thermally conductive filler in the thermally conductive silicone sheet for lithium batteries accounts for 50%-70%.
9. The use of the thermally conductive filler as claimed in claim 8, characterized in that: The preparation of the thermally conductive silicone sheet for lithium batteries comprises the following steps: mixing the silicone rubber substrate and the thermally conductive filler evenly, then adding polymethylphenylsiloxane and octylpolymethylsiloxane and stirring evenly, extruding and molding, and drying.
10. The use of the thermally conductive filler as claimed in claim 9, characterized in that: The silicone rubber substrate is vinyl silicone oil.