Environment-friendly extremely-cold-resistant reclaimed rubber
By introducing cold-resistant reinforcers such as nano zinc oxide, carbon nanotubes, carbon fibers, etc. into rubber recycled rubber, and optimizing the preparation process, the poor performance and pollution problems of recycled rubber in low temperature environments are solved, and the combination of high performance and environmental protection is achieved. , suitable for applications in extremely cold areas.
Patent Information
- Application Number
- CN202411335214.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-12
AI Technical Summary
The existing rubber regeneration technology has high energy consumption, heavy pollution, unstable quality of recycled rubber and poor performance in low temperature environments, making it difficult to meet the requirements of modern industry for environmental protection, high efficiency and high performance, especially in extremely cold areas. satisfy.
New cold-resistant enhancers such as nano zinc oxide, carbon nanotubes, and carbon fiber are prepared in combination with optimized preparation technology to prepare environmentally friendly extremely cold-resistant recycled glue to improve its mechanical properties and flexibility in low temperature environments, while reducing production and use processes. VOCs emissions in.
It significantly improves the performance of recycled glue in low-temperature environments, maintains excellent performance under normal temperature conditions, meets the application needs of extremely cold areas, and reduces environmental pollution, achieving effective utilization of waste resources and reducing production costs.
Smart Images

Figure CN118931000A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of reclaimed rubber, and more specifically, to environmentally friendly extreme cold-resistant reclaimed rubber. Background Art
[0002] With the rapid development of industrialization and the automobile industry, the amount of waste rubber (such as waste tires) generated has increased dramatically, becoming a global environmental problem. If these waste rubbers are not effectively treated, they will seriously pollute the land, water and air, and even cause safety hazards such as fires. According to relevant statistics, the number of waste tires generated in my country each year is huge, and it is increasing year by year. How to deal with these waste rubbers efficiently and environmentally friendly has become an urgent problem to be solved.
[0003] At present, although rubber recycling technology has made certain progress, it still has many limitations. Traditional regeneration methods often have problems such as high energy consumption, heavy pollution, and unstable quality of recycled rubber. It is difficult to meet the requirements of modern industry for environmental protection, high efficiency and high performance. At the same time, traditional recycled rubber has poor performance in low temperature environments and is difficult to meet application requirements in extremely cold areas or extreme weather conditions.
[0004] In view of the above situation, the present invention provides an environmentally friendly extreme cold resistant recycled rubber. By introducing new cold-resistant enhancers such as nano zinc oxide, carbon nanotubes, carbon fibers, etc., combined with an optimized preparation process, the mechanical properties and flexibility of the recycled rubber in a low temperature environment are significantly improved while maintaining its excellent performance under normal temperature conditions. In addition, VOCs emissions during the production and use processes are reduced, thereby reducing the impact on the environment. Summary of the invention
[0005] In order to overcome the above-mentioned defects of the prior art, the present invention provides an environmentally friendly extreme cold-resistant recycled rubber to solve the problems raised in the above-mentioned background technology.
[0006] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: environmentally friendly extreme cold resistant recycled rubber, specifically comprising the following components and weight portions: 60-70 parts of waste tire recycled rubber powder, 10-20 parts of EPDM rubber, 5-10 parts of low-phenyl silica gel, 5-10 parts of cold resistance enhancer, 5-13 parts of environmentally friendly plasticizer and softener, 3-7 parts of filler and stabilizer, and 3-8 parts of other additives.
[0007] Preferably, the recycled rubber powder from waste tires is strictly screened, washed and dried, and the particle size is controlled at 0.8-1.0 mm to ensure the quality of the recycled rubber.
[0008] Preferably, the ethylene content of the EPDM rubber is 40%-50%, and the phenyl content of the low-phenyl silica gel is ≤10%.
[0009] Preferably, the cold resistance enhancer specifically includes nano zinc oxide, carbon nanotubes and carbon fibers, wherein the purity of nano zinc oxide is ≥99.9%, the particle size is 10-30nm, the diameter of carbon nanotubes is 2-20nm, the length is 5-15μm, the strength of carbon fibers is Grade I, and the tensile strength is ≥4900MPa.
[0010] Preferably, the environmentally friendly plasticizer is Sanepar 756 environmentally friendly plasticizer, and the softener is medium viscosity naphthenic oil.
[0011] Preferably, the filler is nano-silicon dioxide and white carbon black, the stabilizer is an antioxidant, and the other additives are any one of n-butyl carbamate and phenolic resin.
[0012] The present invention also provides a preparation method for preparing the above-mentioned environmentally friendly extreme cold resistant reclaimed rubber, and the preparation method specifically comprises the following steps: S1, pretreatment, crushing, screening, washing and drying the waste tires to obtain waste tire recycled rubber powder with a particle size of 0.8-1.0 mm; S2, mixing, the pre-treated waste tire recycled rubber powder, EPDM rubber, low phenyl silica gel, nano zinc oxide, carbon nanotubes, carbon fiber, white carbon black and nano silicon dioxide solid materials are uniformly mixed in a high-speed mixer for 5-10 minutes to ensure that the components are fully dispersed; S3, plasticization, add Sanepar756 environmentally friendly plasticizer and medium viscosity naphthenic oil to the evenly mixed solid material, continue mixing, so that the plasticizer and oil can fully penetrate into the rubber matrix to improve the plasticity and processing performance of the material; S4, desulfurization and regeneration, the plasticized rubber is sent to a mechanical mixer for desulfurization and regeneration, the rotor speed is set to 60-80RPM, the operating temperature is 230-250℃, the pressure is 1.24MPa, and the processing time is 10-15min; S5, extrusion molding, feeding the desulfurized and regenerated rubber into a rubber extruder for extrusion molding to form a semi-finished product of desired shape and size; S6, vulcanization treatment, the extruded semi-finished product is vulcanized to further enhance the cross-linking density and physical properties of the material.
[0013] Preferably, in step S1, specifically, a large crusher is used to crush the waste tires into small pieces, and rubber blocks with a particle size of 6-8 mm are screened out through a vibrating screen, the rubber blocks are cleaned for 35 minutes to remove surface sand and impurities, and air-dried at 60-80°C for 1-2 hours until the moisture content is less than 2%, and the dried rubber blocks are sent to a smooth roller crusher, the roller spacing is controlled to be about 1 mm, and the rubber blocks are crushed into rubber powder with a particle size of 0.8-1.0 mm.
[0014] Preferably, in step S3, the temperature is gradually raised to 100-120°C during the mixing process to allow the plasticizer and oil to better penetrate into the rubber matrix, and the stirring speed is 120-160 r / min.
[0015] Preferably, in step S6, the vulcanization temperature is 120-150°C, the vulcanization time is 5-20 minutes, and the vulcanization pressure is 5 MPa-30 MPa.
[0016] Technical effects and advantages of the present invention: 1. The present invention can maintain good mechanical properties and flexibility in extremely cold environments by adding specific cold-resistant enhancers, such as nano zinc oxide, carbon nanotubes and carbon fibers, thereby improving the performance of recycled rubber in extremely cold environments, ensuring the strength and flexibility of the material at low temperatures, and broadening its application range in cold areas or extreme weather conditions; 2. The present invention reasonably mixes waste tire recycled rubber powder, EPDM rubber, low-phenyl silica gel and other base materials, and optimizes the preparation process, so that the recycled rubber of the present invention also exhibits excellent tensile strength and elongation at break under normal temperature conditions, meeting the application scenarios with high requirements for material strength; 3. The present invention adopts environmentally friendly plasticizers and softeners, which reduces VOCs emissions during production and use, reduces environmental pollution, and meets the pursuit of green and sustainable development by modern industry; 4. The present invention uses waste such as waste tires as the main raw materials and is prepared through advanced recycling technology, which realizes the effective utilization of waste resources, reduces the exploitation of primary resources, reduces production costs, and also contributes to environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 It is the overall flow chart of the present invention. DETAILED DESCRIPTION
[0018] Embodiment 1, This embodiment provides an environmentally friendly extreme cold resistant recycled rubber, which specifically includes the following components and weight parts: 65 parts of waste tire recycled rubber powder, 15 parts of EPDM rubber, 7.5 parts of low-phenyl silica gel, 7.5 parts of cold resistance enhancer, 7 parts of environmentally friendly plasticizer, 6 parts of softener, 5 parts of filler, 3 parts of stabilizer and 4 parts of other additives; The cold resistance enhancer specifically includes 3 parts of nano zinc oxide, 2 parts of carbon nanotubes, and 2.5 parts of carbon fibers.
[0019] This embodiment also provides a preparation method for preparing the above-mentioned environmentally friendly extreme cold resistant reclaimed rubber, and the specific preparation method comprises the following steps: S1, pretreatment, crushing, screening, washing and drying the waste tires to obtain waste tire recycled rubber powder with a particle size of 0.8-1.0 mm; S2, mixing, the pre-treated waste tire recycled rubber powder, EPDM rubber, low phenyl silica gel, nano zinc oxide, carbon nanotubes, carbon fiber, white carbon black and nano silicon dioxide are uniformly mixed in a high-speed mixer for 8 minutes to ensure that the components are fully dispersed; S3, plasticization, add Sanepar756 environmentally friendly plasticizer and medium viscosity naphthenic oil to the uniformly mixed solid material, gradually raise the temperature to 110°C during the mixing process, and stir at a speed of 140r / min to allow the plasticizer and oil to fully penetrate into the rubber matrix; S4, desulfurization and regeneration, the plasticized rubber material is sent to a mechanical mixer for desulfurization and regeneration, the rotor speed is set to 70RPM, the operating temperature is 240℃, the pressure is 1.24MPa, and the processing time is 12min; S5, extrusion molding, feeding the desulfurized and regenerated rubber into a rubber extruder for extrusion molding to form a semi-finished product of desired shape and size; S6. Vulcanization treatment, the vulcanization temperature is 135°C, the vulcanization time is 10 minutes, and the vulcanization pressure is 15 MPa, so as to further enhance the crosslinking density and physical properties of the material.
[0020] Embodiment 2, This embodiment provides an environmentally friendly extreme cold resistant recycled rubber, which specifically includes the following components and weight parts: 70 parts of waste tire recycled rubber powder, 10 parts of EPDM rubber, 10 parts of low-phenyl silica gel, 10 parts of cold-resistant enhancer, 10 parts of environmentally friendly plasticizer, 8 parts of softener, 6 parts of filler, 4 parts of stabilizer and 6 parts of other additives; The cold resistance enhancer specifically includes 4 parts of nano zinc oxide, 3 parts of carbon nanotubes and 3 parts of carbon fibers.
[0021] This embodiment also provides a preparation method for preparing the above-mentioned environmentally friendly extreme cold resistant reclaimed rubber, and the specific preparation method comprises the following steps: S1, pretreatment, the same as in Example 1; S2, mixing, the mixing time is adjusted to 10 minutes; S3, plasticization, gradually raise the temperature to 120°C during mixing, and the stirring speed is 160r / min; S4, desulfurization regeneration, set the rotor speed to 80RPM, the operating temperature to 250℃, and the processing time to 15min; S5, extrusion molding, the same as in Example 1; S6. Vulcanization treatment: the vulcanization temperature is 150°C, the vulcanization time is 15 minutes, and the vulcanization pressure is 20 MPa.
[0022] Embodiment 3, This embodiment provides an environmentally friendly extreme cold resistant recycled rubber, which specifically includes the following components and weight parts: 60 parts of waste tire recycled rubber powder, 20 parts of EPDM rubber, 5 parts of low-phenyl silica gel, 5 parts of cold-resistant enhancer, 5 parts of environmentally friendly plasticizer, 5 parts of softener, 3 parts of filler, 3 parts of stabilizer and 3 parts of other additives; The cold resistance enhancer specifically includes 2 parts of nano zinc oxide, 1 part of carbon nanotubes and 2 parts of carbon fibers.
[0023] This embodiment also provides a preparation method for preparing the above-mentioned environmentally friendly extreme cold resistant reclaimed rubber, and the specific preparation method comprises the following steps: S1, pretreatment, the same as in Example 1; S2, mixing, the mixing time is adjusted to 5 minutes; S3, plasticization, gradually raise the temperature to 100°C during mixing, and the stirring speed is 120r / min; S4, desulfurization regeneration, set the rotor speed to 60RPM, the operating temperature to 230℃, and the processing time to 10min; S5, extrusion molding, the same as in Example 1 and Example 2; S6, vulcanization treatment, the vulcanization temperature is 120℃, the vulcanization time is 5min, and the vulcanization pressure is 5MPa.
[0024] The following is a performance test of the environmentally friendly extreme cold resistant reclaimed rubber prepared in the above embodiment and the existing product (comparative example), and the test method is as follows: 1. Cold resistance test: Low temperature brittleness test: keep the sample in a low temperature environment of -60℃ for 24 hours, and then observe and record whether the sample has cracks or breaks; Low temperature tensile test: at -40℃, the sample is subjected to tensile test using a universal material testing machine to measure its tensile strength, elongation at break and other parameters, and compared with the test results at room temperature; 2. Physical performance test: Hardness test: use Shore hardness tester to measure the hardness value of the sample; Density test: Determine the density of the sample using the water displacement method or the pycnometer method; Resilience test, using a resilience tester to measure the sample's ability to recover after a certain compression; 3. Mechanical strength test: Tensile strength test: Under normal temperature conditions, use a universal material testing machine to perform a tensile test on the sample to measure its tensile strength, elongation at break and other parameters; The tear strength test uses the right-angle tear test method to measure the maximum force of the sample during the tearing process; Compression set test: After placing the sample under a certain pressure for a certain period of time, its compression set rate is measured; 4. Environmental protection test: Volatile organic compound (VOCs) emission test, placing the sample in a specific environment, collecting and detecting the VOCs content released; Heavy metal content test, using atomic absorption spectrometry or inductively coupled plasma mass spectrometry (ICP-MS) and other methods to detect the content of heavy metal elements in the sample; Biodegradability testing, under specific conditions, evaluates the biodegradability of samples in the natural environment; 5. Practical application test Simulate extreme cold environment application test, make the sample into a specific shape (such as tires, sealing strips, etc.), conduct actual application test in simulated extreme cold environment (such as below -40℃), observe and record its performance; Durability testing: Under conditions simulating actual use, samples are subjected to long-term operation or cyclic loading tests to evaluate their durability and service life.
[0025] The specific test data are shown in the following table: According to the above table data, the environmentally friendly extreme cold resistant reclaimed rubber of the present invention performs well in multiple key performance indicators, including tensile strength, elongation at break, tensile strength and elongation at break at low temperature, and environmental protection (low VOCs emission). These data show that the reclaimed rubber of the present invention not only has excellent mechanical properties, can maintain high strength and flexibility at room temperature and low temperature environment, but also has good environmental protection characteristics, reducing pollution to the environment; The comparative examples are lower than the examples of the present invention in all performance indicators, especially in low temperature performance and environmental protection. This further verifies the important role of the specific ingredients added by the present invention (such as cold-resistant enhancers, environmentally friendly plasticizers, etc.) in improving the performance of reclaimed rubber. In summary, the environmentally friendly extreme cold-resistant recycled rubber of the present invention successfully achieves an organic combination of high performance and environmental protection through reasonable formula design and preparation process, and provides a new type of material with broad application prospects for related fields.
[0026] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. Environmentally friendly extreme cold resistant recycled rubber, characterized by: Specifically, it includes the following ingredients and weight proportions: 60-70 parts of recycled rubber powder from waste tires, 10-20 parts of EPDM rubber, 5-10 parts of low-phenyl silica gel, 5-10 parts of cold-resistant enhancer, 5-13 parts of environmentally friendly plasticizer and softener, 3-7 parts of filler and stabilizer, and 3-8 parts of other additives.
2. The environmentally friendly extreme cold resistant reclaimed rubber according to claim 1, characterized in that: The waste tire recycled rubber powder is strictly screened, washed and dried, and the particle size is controlled at 0.8-1.0mm to ensure the quality of the recycled rubber.
3. The environmentally friendly extreme cold resistant reclaimed rubber according to claim 2, characterized in that: The ethylene content of the EPDM rubber is 40%-50%, and the phenyl content of the low-phenyl silica gel is ≤10%.
4. The environmentally friendly extreme cold resistant reclaimed rubber according to claim 3, characterized in that: The cold resistance enhancer specifically includes nano zinc oxide, carbon nanotubes and carbon fibers, wherein the purity of nano zinc oxide is ≥99.9%, the particle size is 10-30nm, the diameter of carbon nanotubes is 2-20nm, the length is 5-15μm, the strength of carbon fibers is Grade I, and the tensile strength is ≥4900MPa.
5. The environmentally friendly extreme cold resistant reclaimed rubber according to claim 4, characterized in that: The environmentally friendly plasticizer is Sanepar 756 environmentally friendly plasticizer, and the softener is medium-viscosity naphthenic oil.
6. The environmentally friendly extreme cold resistant reclaimed rubber according to claim 5, characterized in that: The filler is nano silicon dioxide and white carbon black, the stabilizer is an antioxidant, and the other additives are any one of n-butyl carbamate and phenolic resin.
7. A preparation method for preparing the environmentally friendly extreme cold resistant reclaimed rubber according to claim 6, characterized in that: The preparation method specifically comprises the following steps: S1, pretreatment, crushing, screening, washing and drying the waste tires to obtain waste tire recycled rubber powder with a particle size of 0.8-1.0 mm; S2, mixing, the pre-treated waste tire recycled rubber powder, EPDM rubber, low phenyl silica gel, nano zinc oxide, carbon nanotubes, carbon fiber, white carbon black and nano silicon dioxide solid materials are uniformly mixed in a high-speed mixer for 5-10 minutes to ensure that the components are fully dispersed; S3, plasticization, add Sanepar756 environmentally friendly plasticizer and medium viscosity naphthenic oil to the evenly mixed solid material, continue mixing, so that the plasticizer and oil can fully penetrate into the rubber matrix to improve the plasticity and processing performance of the material; S4, desulfurization and regeneration, the plasticized rubber is sent to a mechanical mixer for desulfurization and regeneration, the rotor speed is set to 60-80RPM, the operating temperature is 230-250℃, the pressure is 1.24MPa, and the processing time is 10-15min; S5, extrusion molding, feeding the desulfurized and regenerated rubber into a rubber extruder for extrusion molding to form a semi-finished product of a desired shape and size; S6, vulcanization treatment, the extruded semi-finished product is vulcanized to further enhance the cross-linking density and physical properties of the material.
8. The preparation method according to claim 7, characterized in that: In step S1, specifically, a large crusher is used to crush the waste tires into small pieces, and rubber blocks with a particle size of 6-8 mm are screened out through a vibrating screen. The rubber blocks are washed for 35 minutes to remove surface sand and impurities, and air-dried at 60-80°C for 1-2 hours until the moisture content is less than 2%. The dried rubber blocks are sent to a smooth roller crusher, the roller spacing is controlled to be about 1 mm, and the rubber blocks are crushed into rubber powder with a particle size of 0.8-1.0 mm.
9. The preparation method according to claim 7, characterized in that: In step S3, the temperature is gradually raised to 100-120°C during the mixing process to allow the plasticizer and oil to better penetrate into the rubber matrix, and the stirring speed is 120-160r / min.