Lining layer material and application thereof
By blending and extruding with high-density polyethylene, the antibacterial barrier material is formed, and the problem of insufficient gas barrier properties and antibacterial properties of the inner lining layer material of the oil and gas transport composite pipe is solved, and better gas is achieved Barrier and antibacterial properties reduce the risk of pipeline blockage and difficulty in cleaning pipes.
Patent Information
- Application Number
- CN202310531850.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
The gas barrier properties and antibacterial properties of the inner lining layer materials of the existing oil and gas delivery composite pipes are insufficient, resulting in gas penetration and bacterial adhesion, increasing the risk of pipeline blockage and difficulty in cleaning pipes.
Modified nanofillers and antibacterial agents are blended and extruded with high-density polyethylene. The dispersion and compatibility of nanofillers and coupling agents are improved by cationic surfactant modification of nanofillers and coupling agents, forming antibacterial barrier materials and enhancing gas barriers and antibacterial properties.
It significantly improves the gas barrier and antibacterial properties of the inner lining layer, reduces gas permeability and bacterial adhesion, reduces the frequency and cost of pipe cleaning, and enhances the interlayer binding strength.
Smart Images

Figure CN118931003A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of oil and gas transmission pipelines, and in particular to an inner lining material and application thereof. Background Art
[0002] With the development of oil and gas resources, fiber reinforced composite pipe (RTP) is widely used in the field of oil and gas gathering and transportation due to its advantages such as light weight, flexible coiling and corrosion resistance. RTP pipe is usually composed of three layers: an inner lining layer made of polymer material, a reinforcement layer made of continuous fiber material, and an outer pipe made of anti-aging and impact thermoplastic plastic. The main function of the inner lining layer is to seal the conveying material and prevent leakage; the main function of the reinforcement layer is to provide the required pressure bearing capacity of the pipe body; the main function of the outer pipe is to protect the entire pipe body. The inner lining material plays a key role in the quality of the composite pipe.
[0003] The lining material of RTP pipe is generally made of high-density polyethylene (HDPE). HDPE has good anti-seepage performance against water vapor. However, oil and gas gathering and transportation are usually medium- and high-pressure oil and gas, which often contain small molecular permeable media such as oxygen, carbon dioxide, hydrogen sulfide, and methane. HDPE has poor anti-seepage performance against gases such as oxygen, carbon dioxide, hydrogen sulfide, and methane in high-pressure oil and gas. If the anti-permeability of the lining layer is insufficient, these media will penetrate into the middle reinforcement layer, causing the hydrolysis and corrosion failure of the reinforcement layer material, and the collapse and failure of the entire pipeline during rapid pressure relief. In addition, the oil and gas in oil and gas gathering and transportation often contain bacteria. The bacteria adhere to and multiply on the pipe wall for a long time, which will reduce the flow area of the pipeline. In severe cases, it will also cause pipeline blockage. Once blocked, regular cleaning operations must be performed to ensure the normal operation of the pipeline. For high-pressure oil and gas gathering and transportation composite pipes, due to the limitations of pipeline structure, cleaning operations are difficult and costly. Therefore, it is of great significance to develop an inner lining material with good gas barrier properties, anti-interlayer peeling properties, and antibacterial properties.
[0004] Patent application CN202210231254.9 discloses a polymer composite material with high gas barrier properties. The method mechanically mixes graphene oxide with high-density polyethylene, then extrude and granulate, and press into thin sheets to obtain a composite material, which can have a certain barrier property against gas. However, graphene oxide is easy to agglomerate, so its effect on improving the gas barrier property of high-density polyethylene is very limited; and graphene oxide has poor compatibility with high-density polyethylene. As a result, when the composite material is subjected to long-term pulse fluctuations of the pipe fluid, the interface between graphene oxide and polyethylene may produce fatigue aging, resulting in "debonding" phenomenon. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of poor gas barrier properties and antibacterial properties of the lining materials of composite pipes for oil and gas transportation in the prior art, and to provide an lining material and its application. The lining material has good gas barrier properties, resistance to interlayer delamination and antibacterial properties, and can be used in scenarios with high gas barrier requirements.
[0006] In order to achieve the above object, the present invention provides an inner lining material on one hand, wherein the inner lining material contains high-density polyethylene a and an antibacterial barrier material.
[0007] The antibacterial barrier material contains high-density polyethylene b, modified nanofiller, antibacterial agent and a first auxiliary agent, wherein the modified nanofiller is obtained by modifying a sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer;
[0008] Based on the total weight of the antibacterial barrier material, the content of the modified nano filler is 2-6wt%.
[0009] Preferably, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%.
[0010] Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.
[0011] Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0012] Preferably, the modified nanofiller is prepared according to the following process:
[0013] S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;
[0014] S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.
[0015] Preferably, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50.
[0016] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.
[0017] Preferably, the melt index of the high-density polyethylene b is 0.3-0.5 g / 10 min.
[0018] Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide.
[0019] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0020] Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0021] Preferably, the antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are blended and extruded.
[0022] Preferably, the blending extrusion is carried out in a twin-screw extruder.
[0023] Preferably, the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
[0024] Preferably, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%.
[0025] Preferably, the high-density polyethylene a and the high-density polyethylene b are the same.
[0026] Preferably, the inner lining material further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.
[0027] Preferably, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
[0028] A second aspect of the present invention provides a method for preparing an inner lining layer, the method comprising:
[0029] A1, blending and extruding high-density polyethylene b, modified nanofiller, antibacterial agent and first auxiliary agent, cooling and granulating to obtain antibacterial barrier material;
[0030] A2, blending and extruding the antibacterial barrier material and high-density polyethylene a;
[0031] Wherein, in step A1, the modified nanofiller is obtained by modifying a flaky nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
[0032] Preferably, in step A1, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%.
[0033] Preferably, in step A1, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
[0034] Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite.
[0035] Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0036] Preferably, the melt index of the high-density polyethylene b is 0.3-0.5 g / 10 min.
[0037] Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide.
[0038] Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0039] Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0040] Preferably, the method further comprises preparing the modified nanofiller according to the following steps:
[0041] The water is heated to 70-90° C., and then mixed with the flaky nanofiller to obtain a mixture;
[0042] The pH of the mixture is adjusted to 6.8-7.5 and continued to be heated for 30-50 minutes, and then reacted with a cationic surfactant, the obtained reaction liquid is separated into solid and liquid, and then the obtained solid is washed, dried, ground and sieved.
[0043] Preferably, in step A2, the blending extrusion is carried out in a twin-screw extruder.
[0044] Preferably, in step A2, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 110-130°C, the temperature of zone two is 140-160°C, and the temperature of zone three is 180-200°C.
[0045] Preferably, in step A2, the head temperature of the twin-screw extruder is 165-185°C.
[0046] Preferably, in step A2, based on the total weight of the antibacterial barrier material and the high-density polyethylene a, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%.
[0047] Preferably, the high-density polyethylene a and the high-density polyethylene b are the same.
[0048] Preferably, step A2 comprises: co-extruding the antibacterial barrier material, high-density polyethylene a and a second auxiliary agent, wherein the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.
[0049] Preferably, in step A2, based on the total weight of the high-density polyethylene a, the antibacterial barrier material and the second auxiliary agent, the content of the second auxiliary agent is 1-2 wt %.
[0050] A third aspect of the present invention provides a composite pipe, the composite pipe comprising an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside;
[0051] The inner lining layer is made of the inner lining layer material described above.
[0052] Preferably, the reinforcement layer is made of continuous fiber reinforced resin prepreg tapes wound around the outer side of the inner liner in a cross manner.
[0053] Preferably, the outer tube is made of a raw material containing medium-density polyethylene or low-density polyethylene.
[0054] Preferably, the melt index of the medium density polyethylene or low density polyethylene is
[0055] 0.5~0.7g / 10min.
[0056] Preferably, the raw material for preparing the outer tube further contains a third auxiliary agent, wherein the third auxiliary agent is selected from one or more of a plasticizer, a flame retardant, an antioxidant, a masterbatch and an anti-ultraviolet agent.
[0057] Compared with the prior art, the technical solution of the present invention has the following advantages:
[0058] 1. The present invention improves the dispersibility of the flaky nanofiller in high-density polyethylene (including high-density polyethylene a and high-density polyethylene b) by modifying the flaky nanofiller, so that the flaky nanofiller can better improve the gas barrier property of the antibacterial barrier material;
[0059] 2. The present invention improves the compatibility of high-density polyethylene and modified nanofiller by adding the first auxiliary agent, so that high-density polyethylene can be better combined with the modified nanofiller, thereby avoiding the "debonding" phenomenon of the modified nanofiller; at the same time, the addition of the first auxiliary agent can also improve the bonding between the lining layer material and the reinforcement layer material, thereby improving its anti-interlayer peeling property;
[0060] 3. The present invention improves the dispersibility of the antibacterial agent in high-density polyethylene by adding the modified nanofiller and the first auxiliary agent, so that the antibacterial agent can better exert its antibacterial properties, thereby preventing bacteria in the oil and gas production fluid from adhering to the pipe wall;
[0061] 4. The present invention first prepares an antibacterial barrier material with high-density polyethylene b, modified nanofiller, antibacterial agent and a first auxiliary agent, and then prepares an inner lining layer with high-density polyethylene a. This can further improve the dispersibility of the nanofiller and the antibacterial agent in the high-density polyethylene, and make the modified nanofiller and the antibacterial agent uniformly dispersed in the high-density polyethylene, thereby making the gas barrier and antibacterial properties of the inner lining layer excellent, and can be well applied to medium and high pressure oil and gas transportation scenarios. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] Figure 1 is a schematic structural diagram of an embodiment of the composite tube of the present invention;
[0063] Figure 2 Schematic diagram of the microscopic morphology of the inner lining layer prepared in Comparative Example 6 of the present invention;
[0064] Figure 3 is a schematic diagram of the microscopic morphology of the lining layer prepared in Example 1 of the present invention;
[0065] Figure 4 is a test curve diagram of interlayer bonding strength of the composite pipe prepared in Example 7 of the present invention;
[0066] Figure 5 It is a test curve diagram of interlayer bonding strength of the composite pipe prepared in Comparative Example 7 of the present invention.
[0067] Description of Reference Numerals
[0068] 1. Inner lining layer; 2. Reinforcement layer; 3. Outer tube. DETAILED DESCRIPTION
[0069] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0070] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0071] The inner lining material described in the present invention contains high-density polyethylene a and an antibacterial barrier material, wherein the antibacterial barrier material contains high-density polyethylene b, modified nanofiller, an antibacterial agent and a first auxiliary agent, and the modified nanofiller is obtained by modifying a flaky nanofiller with a cationic surfactant; based on the total weight of the antibacterial barrier material, the content of the modified nanofiller is 2 to 6 wt%.
[0072] In the present invention, the first auxiliary agent is a coupling agent and / or a compatibilizer, preferably a coupling agent and a compatibilizer.
[0073] The inner lining material described in the present invention enables the antibacterial agent to be evenly dispersed in the high-density polyethylene under the action of the modified nano filler and the first auxiliary agent, so that the antibacterial agent can fully exert its antibacterial performance, so that the bacteria in the oil and gas transmission medium will not adhere to the pipe wall, avoiding pipeline blockage caused by bacterial growth on the pipe wall, reducing the frequency of pipeline cleaning operations and reducing pipeline cleaning costs.
[0074] In a preferred embodiment, based on the total weight of the inner lining material (i.e., based on the total weight of the raw materials for preparing the inner lining material), the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%. More preferably, based on the total weight of the inner lining material, the content of the high-density polyethylene a is 85-95wt%, and the content of the antibacterial barrier material is 5-15wt%.
[0075] In a preferred embodiment, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%. Within the above range, the obtained lining material has better antibacterial and gas barrier properties and low cost.
[0076] If the flaky nanofiller is added directly, it is easy to agglomerate, so that the flaky nanofiller cannot be distributed in the polyethylene in a flaky manner, thereby making the gas barrier property of the liner material poor. The present invention further improves its dispersibility in the resin matrix by modifying the flaky nanofiller. In a preferred embodiment, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, more preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0077] In order to make the modified nanofiller more dispersible in high-density polyethylene (i.e., resin matrix), in a preferred embodiment, the flaky nanofiller is a layered nanomaterial with a large aspect ratio, specifically, it can be one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite, preferably montmorillonite.
[0078] In a preferred embodiment, the modified nanofiller is prepared according to the following process:
[0079] Step S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture;
[0080] Step S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid from the solid-liquid, and then washing, drying, grinding and sieving the obtained solid.
[0081] Wherein, in step S10, the weight ratio of the flaky nanofiller to water is 1:25-50, specifically, for example, 1:25, 1:30, 1:33, 1:35, 1:40, 1:45 or 1:50.
[0082] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20, specifically, for example, 1:10, 1:12, 1:15, 1:17, 1:18 or 1:20.
[0083] In a specific embodiment, step S20 includes: adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then mixing with a cationic surfactant and adjusting the pH value to 6.8-7.5, reacting for 2-4 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3-5 times, then drying at 70-90° C. for 30-50 hours, and finally grinding and sieving.
[0084] In a preferred embodiment, the melt index of the high-density polyethylene b is 0.3 to 0.5 g / 10 min, more preferably 0.35 to 0.45 g / 10 min.
[0085] The present invention does not limit the specific type of the antibacterial agent. Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide, more preferably nano copper oxide and nano silver oxide.
[0086] In a preferred embodiment, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0087] In a preferred embodiment, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0088] In order to improve the antibacterial and gas barrier properties of the lining material, in a preferred embodiment, the antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are co-blended and extruded.
[0089] Further preferably, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
[0090] In order to improve the performance of the inner lining material such as processability and service life, in a preferred embodiment, the inner lining material further contains a second auxiliary agent, which is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.
[0091] Furthermore, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
[0092] In a preferred embodiment, in the inner lining material, the content of the high-density polyethylene a is 85-95wt%, the content of the antibacterial barrier material is 4-14wt%, and the content of the second auxiliary agent is 1-2wt%. In this way, the overall performance of the obtained inner lining material is better.
[0093] In the present invention, the high-density polyethylene a and the high-density polyethylene b may be the same or different, and are preferably the same for better compatibility and ease of operation.
[0094] The present invention also provides a method for preparing an inner lining layer, the method comprising:
[0095] Step A1, blending and extruding high-density polyethylene b, modified nanofiller, antibacterial agent and first auxiliary agent, cooling and granulating to obtain antibacterial barrier material;
[0096] Step A2, blending and extruding the antibacterial barrier material and high-density polyethylene a to obtain an inner lining layer;
[0097] Wherein, in step A1, the modified nanofiller is obtained by modifying a flaky nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
[0098] In the present invention, the antibacterial barrier material is first prepared by co-extruding high-density polyethylene b, modified nanofiller, antibacterial agent and the first auxiliary agent, and then co-extruding with high-density polyethylene a (matrix) to prepare the inner lining layer. The dispersibility of the nanofiller and the antibacterial agent in the high-density polyethylene can be further improved, and the modified nanofiller and the antibacterial agent can be evenly dispersed in the high-density polyethylene, thereby making the gas barrier and antibacterial properties of the inner lining layer excellent.
[0099] In the inner liner prepared by the method described in the present invention, the modified nano filler and the antibacterial agent are uniformly dispersed in the HDPE, and the HDPE matrix tightly wraps the modified nano filler and the antibacterial agent particles without holes. Compared with the inner liner made of pure HDPE, the gas permeability of the inner liner is reduced by about 100 times, which essentially reduces the total amount of gas infiltrating into the composite pipe. At the same time, the inner liner has excellent antibacterial properties against bacteria in oil and gas. Therefore, the inner liner has obvious competitive advantages when used as the inner liner of the medium and high pressure oil and gas transmission composite pipe.
[0100] In a preferred embodiment, in step A1, based on the total weight of the antibacterial barrier material (that is, based on the total weight of the raw materials for preparing the antibacterial barrier material), the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%.
[0101] In the specific implementation, in step A1, the blending extrusion is carried out in a twin-screw extruder. Preferably, the working temperature of the twin-screw extruder is 160-200°C, the working speed is 300-350r / min, and the working time is 3-6min. Specifically, the working temperature of the twin-screw extruder is divided into three sections along the screw extrusion direction, the temperature of the first section is 160-170°C, the temperature of the second section is 175-185°C, and the temperature of the third section is 190-200°C.
[0102] In the method described in the present invention, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite. Compared with other flaky nanofillers, the above flaky nanofiller has better dispersibility in high-density polyethylene.
[0103] In the method of the present invention, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
[0104] In the method of the present invention, the melt index of the high-density polyethylene b is 0.3 to 0.5 g / 10 min, more preferably 0.35 to 0.45 g / 10 min.
[0105] In the method of the present invention, the antibacterial agent is nano copper oxide and / or nano silver oxide, preferably nano copper oxide and nano silver oxide.
[0106] In the method of the present invention, the compatibilizer is selected from one or more of maleic anhydride grafted high density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer.
[0107] In the method of the present invention, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
[0108] The method of the present invention also includes preparing the modified nanofiller according to the following steps:
[0109] (1) heating water to 70-90° C. and then mixing water with the flaky nanofiller to obtain a mixture;
[0110] (2) adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.
[0111] Wherein, in step (1), the weight ratio of the flaky nanofiller to water is 1:25-50, specifically, for example, 1:25, 1:30, 1:33, 1:35, 1:40, 1:45 or 1:50.
[0112] Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20, specifically, for example, 1:10, 1:12, 1:15, 1:17, 1:18 or 1:20.
[0113] In a specific embodiment, step (2) comprises: adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then mixing with a cationic surfactant and adjusting the pH value to 6.8-7.5, reacting for 2-4 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3-5 times, then drying at 70-90° C. for 30-50 hours, and finally grinding and sieving.
[0114] In the method described in the present invention, the blending extrusion operation in step A2 is carried out in a twin-screw extruder; wherein the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one (the temperature of the rear part of the body) is 110-130°C, the temperature of zone two (the temperature of the middle part of the body) is 140-160°C, and the temperature of zone three (the temperature of the front part of the body) is 180-200°C.
[0115] Furthermore, in step A2, the die head temperature of the twin-screw extruder is 165-185° C. Specifically, the die head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 175-185° C., and the die temperature is 165-175° C.
[0116] In the method described in the present invention, in step A2, based on the total weight of the antibacterial barrier material and high-density polyethylene a, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%; preferably, the content of the high-density polyethylene a is 85-95wt%, and the content of the antibacterial barrier material is 5-15wt%.
[0117] In the method described in the present invention, the high-density polyethylene a and the high-density polyethylene b may be the same or different, and are preferably the same for better compatibility and ease of operation.
[0118] In the method described in the present invention, step A2 comprises: co-extruding the antibacterial barrier material, high-density polyethylene a and a second auxiliary agent, wherein the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent.
[0119] In the method described in the present invention, in step A2, based on the total weight of the high-density polyethylene a, the antibacterial barrier material and the second auxiliary agent, the content of the second auxiliary agent is 1-2 wt %.
[0120] The present invention also proposes a composite pipe, please refer to Figure 1 The composite pipe comprises an inner lining layer 1, a reinforcement layer 2 and an outer pipe 3 which are arranged in sequence from the inside to the outside; the inner lining layer 1 is made of the inner lining layer material as described above or is made by the method as described above.
[0121] The composite pipe can be used for transporting high-pressure oil and gas, and the high-pressure oil and gas contain produced fluid.
[0122] In a specific embodiment, the thickness of the inner lining layer 1 is 2 to 10 mm.
[0123] In a specific implementation, the thickness of the outer tube 3 is 2-4 mm.
[0124] In the composite pipe of the present invention, the reinforcement 2 is wound on the outer side of the inner lining layer 1 in a cross manner by continuous fiber reinforced resin prepreg tape. The number of winding layers of the reinforcement layer 2 is determined according to the pressure level of the composite pipe. Specifically, the number of winding layers can be an even number of 2 to 20 layers, and the calculation method of the number of winding layers refers to SY 6662.2.
[0125] In the composite pipe described in the present invention, the continuous fiber reinforced resin prepreg tape is made of one or more continuous fiber mixed materials of glass fiber, aramid fiber, carbon fiber and the same material of polymer polyolefin (matrix) of the inner lining layer 1 through prepreg process. The reinforcing resin in the reinforcing layer 2 has good bonding performance with the inner lining layer made of the inner lining material, and the bonding is reliable, so that the reinforcing layer 2 and the inner lining layer 1 are integrated, the anti-peeling performance between the reinforcing layer 2 and the inner lining layer is improved, and the winding defects between the reinforcing layer 2 and the inner lining layer 1 are effectively avoided, thereby reducing the possibility of delamination of the inner lining layer 1 and the reinforcing layer 2 caused by the accumulation of oil and gas in the defective part after the pipeline penetrates into the pipe body; at the same time, because the inner lining layer 1 material and the reinforcing layer 2 material are of the same material, the thermal shrinkage rate is almost the same, and the internal stress formed inside the pipe wall by the temperature change of the pipeline is small, which can greatly improve the ability of the composite pipe to withstand pressure and reduce the probability of damage to the composite pipe.
[0126] In the composite pipe of the present invention, the outer pipe 3 is made of a raw material containing medium-density polyethylene or low-density polyethylene. The permeability of the outer pipe 3 is higher than that of the inner lining material, and the composite pipe forms a structure with gradually decreasing gas barrier properties from the inside to the outside, so that the gas that penetrates into the composite pipe is more likely to penetrate from the pipe to the outside, thereby avoiding the gas that penetrates into the pipe to gather in the pipe and cause interlayer peeling.
[0127] In the composite tube of the present invention, the melt index of the medium-density or low-density polyethylene used to prepare the outer tube 3 is 0.5 to 0.7 g / 10 min, preferably 0.55 to 0.65 g / 10 min.
[0128] In a preferred embodiment, the raw material for preparing the outer tube 3 further contains a third auxiliary agent, wherein the third auxiliary agent is selected from one or more of a plasticizer, a flame retardant, an antioxidant, a masterbatch and an anti-ultraviolet agent. By adding the third auxiliary agent, the outer tube 3 plays the role of aesthetics, antistatic and flame retardancy.
[0129] The present invention does not limit the preparation method of the composite tube, which can be a conventional operation in the art. In a specific embodiment, the method for preparing the composite tube includes the following steps:
[0130] Prepare the inner lining layer 1 according to the method described above;
[0131] After the continuous fiber reinforced resin prepreg is heated by radiation, the continuous fiber prepreg is cross-wound around the outer side of the inner liner 1 at an angle of 40 to 65 degrees with the axis of the inner liner 1 to obtain a reinforcement layer 2;
[0132] The medium-density polyethylene or the low-density polyethylene is blended and extruded through an extruder, and coated on the outside of the reinforcement layer 2 to obtain a composite pipe.
[0133] Specifically, when preparing the outer tube 3, the specific process in the extruder includes: adding the raw materials in proportion to the high-speed mixing barrel of the extruder for mixing, heating the obtained outer tube material particles, injection molding and placing them in a vacuum chamber, and then cooling and shaping and demolding to obtain the outer tube 3.
[0134] The present invention will be described in detail below through examples, but the protection scope of the present invention is not limited thereto.
[0135] Example 1
[0136] This example is used to illustrate the inner lining material and its application (the preparation method of the inner lining) of the present invention. In this example, the high-density polyethylene a and high-density polyethylene b are the same, and the grade is YGH041, and the melt index is 0.4 g / 10 min.
[0137] 1. Preparation of modified nanofillers
[0138] S10, heating deionized water to 80° C., then adding nano-montmorillonite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-montmorillonite to water is 1:25;
[0139] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 minutes, then adding octadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the octadecyltrimethylammonium chloride to the nano-montmorillonite is 1:12), and adjusting the pH value to 7.0-7.2, reacting for 3 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80° C. for 48 hours, and finally grinding and sieving to obtain modified nano-montmorillonite, i.e., modified nano-filler.
[0140] 2. Preparation of antibacterial barrier materials
[0141] A11, weighing the raw material components according to the following weight percentages: 87wt% of high-density polyethylene b, 2wt% of modified nanofiller, 10wt% of antibacterial agent and 1wt% of the first auxiliary agent, wherein the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1, and the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;
[0142] A12. Add the raw material components in step A11 into a twin-screw extruder and mix them evenly, heat the screw extruder, and perform mixing in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section, and a third section along the extrusion direction of the screw. The temperature of the first section is 160° C., the temperature of the second section is 180° C., and the temperature of the third section is 190° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the lining layer material in the twin-screw extruder is 5 min. After being extruded from the twin-screw extruder, the material is cooled and pelletized to obtain an antibacterial barrier material.
[0143] 3. Preparation of lining layer
[0144] A21. Weigh the raw material components according to the following weight percentages: 89 wt% of high-density polyethylene a, 10 wt% of antibacterial barrier material and 1 wt% of a second auxiliary agent, wherein the second auxiliary agent is a mixture of a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)benzene propionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) in a weight ratio of 1:1:1;
[0145] A22. Add the raw material components in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0146] Example 2
[0147] The method described in Example 1 is used for implementation, except that the preparation of the antibacterial barrier material is as follows:
[0148] A11, weighing the raw material components according to the following weight percentages: 88wt% of high-density polyethylene b, 3wt% of modified nano filler, 8wt% of antibacterial agent and 1wt% of the first auxiliary agent, wherein the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1, and the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1;
[0149] A12. Add the raw material components in step A11 into a twin-screw extruder and mix them evenly, heat the screw extruder, and perform mixing in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section, and a third section along the extrusion direction of the screw. The temperature of the first section is 170° C., the temperature of the second section is 185° C., and the temperature of the third section is 200° C. The extruder speed of the twin-screw extruder is 300 r / min, and the total residence time of the lining layer material in the twin-screw extruder is 5 min. After being extruded from the twin-screw extruder, the material is cooled and pelletized to obtain an antibacterial barrier material.
[0150] Example 3
[0151] This example is used to illustrate the inner lining material and its application (the preparation method of the inner lining) of the present invention. In this example, the high-density polyethylene a and high-density polyethylene b are the same, and the grade is YGH041, and the melt index is 0.4 g / 10 min.
[0152] 1. Preparation of modified nanofillers
[0153] S10, heating deionized water to 85° C., then adding nano-muscovite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-muscovite to water is 1:20;
[0154] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 min, then adding octadecyl dimethyl benzyl ammonium chloride and stirring evenly (the weight ratio of the octadecyl dimethyl benzyl ammonium chloride to the nano muscovite is 1:10), and adjusting the pH value to 7.0-7.2, reacting for 2 h, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80 ° C for 48 h, and finally grinding and sieving to obtain modified nano muscovite, i.e., modified nano filler.
[0155] 2. Preparation of antibacterial barrier materials
[0156] A11, weighing the raw material components according to the following weight percentages: 88wt% of high-density polyethylene b, 5wt% of modified nanofiller, 6wt% of antibacterial agent and 1wt% of the first auxiliary agent; wherein the first auxiliary agent comprises a titanate coupling agent (dioctylphosphite acyloxy titanate) and a compatibilizer (acrylic grafted polyethylene) in a weight ratio of 1:1, and the antibacterial agent comprises nano silver oxide and nano copper oxide in a weight ratio of 2:1;
[0157] A12, adding the raw material components in step A11 into a twin-screw extruder and mixing them evenly, heating the screw extruder, and performing mixing in the twin-screw extruder, wherein the temperature of the twin-screw extruder is divided into a first section, a second section, and a third section, wherein the temperature of the first section is 160° C., the temperature of the second section is 175° C., and the temperature of the third section is 190° C. The extruder speed of the twin-screw extruder is 350 r / min, and the total residence time of the antibacterial barrier material in the twin-screw extruder is 5 min. After being extruded from the twin-screw extruder, the material is cooled and pelletized to obtain an antibacterial barrier material;
[0158] 3. Preparation of lining layer
[0159] A21. Weigh the raw material components according to the following weight percentages: 85 wt% of high-density polyethylene a, 14 wt% of antibacterial barrier material and 1 wt% of a second auxiliary agent; wherein the second auxiliary agent is a mixture of a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) in a weight ratio of 1:1:1;
[0160] A22. Add the raw material components in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0161] Example 4
[0162] This example is used to illustrate the inner lining material and its application (the preparation method of the inner lining) of the present invention. In this example, the high-density polyethylene a and high-density polyethylene b are the same, and the grade is YGH041, and the melt index is 0.4 g / 10 min.
[0163] 1. Preparation of modified nanofillers
[0164] S10, heating deionized water to 75° C., then adding nano hydrated kaolin and stirring evenly to obtain a mixture, wherein the weight ratio of the nano hydrated kaolin to water is 1:30;
[0165] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 minutes, then adding hexadecyltrimethylammonium chloride and stirring evenly (the weight ratio of the hexadecyltrimethylammonium chloride to the nano hydrated kaolin is 1:20), and adjusting the pH value to 7.0-7.2, reacting for 4 hours, filtering the obtained reaction solution, washing the filtered solid with deionized water 4 times, and then drying at 80°C for 48 hours, and finally grinding and sieving to obtain a modified nano kaolin filler.
[0166] 2. Preparation of antibacterial barrier materials
[0167] A11, weighing the raw material components according to the following weight percentages: 81wt% of high-density polyethylene b, 6wt% of modified nanofiller, 9wt% of antibacterial agent and 3wt% of the first auxiliary agent; wherein the first auxiliary agent comprises a silane coupling agent (vinyl triethoxysilane) and a compatibilizer (maleic anhydride grafted high-density ethylene) in a weight ratio of 1:1.5, and the antibacterial agent is nano silver oxide;
[0168] A12. Add the raw material components in step A11 into a twin-screw extruder and mix them evenly, heat the screw extruder, and perform mixing in the twin-screw extruder. The temperature of the twin-screw extruder is divided into a first section, a second section, and a third section. The temperature of the first section is 170°C, the temperature of the second section is 185°C, and the temperature of the third section is 200°C. The extruder speed of the twin-screw extruder is 300r / min, and the total residence time of the lining layer material in the twin-screw extruder is 5min. After being extruded from the twin-screw extruder, the material is cooled and pelletized to obtain an antibacterial barrier material.
[0169] 3. Preparation of lining layer
[0170] A21. Weigh the raw material components according to the following weight percentages: 93 wt% of high-density polyethylene a, 6 wt% of antibacterial barrier material and 1 wt% of a second auxiliary agent; wherein the second auxiliary agent is a mixture of a plasticizer (polyolefin elastomer POE), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and an anti-ultraviolet agent (2-hydroxy-4-n-octyloxybenzophenone) in a weight ratio of 1.5:1.5:1;
[0171] A22. Add the raw material components weighed in step A21 into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 130°C, the temperature of zone two is 160°C, and the temperature of zone three is 200°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 185°C, and the die temperature is 175°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0172] Example 5
[0173] The method described in Example 1 was followed, except that the second auxiliary agent was not added when preparing the inner lining layer;
[0174] Specifically, step A21 is: weigh the raw material components according to the following weight percentages: 90wt% of high-density polyethylene a, 10wt% of antibacterial barrier material.
[0175] Example 6
[0176] The method described in Example 1 is used for implementation, except that the modified nano filler used is modified nano muscovite.
[0177] Specifically, the preparation method of modified nano muscovite comprises the following steps:
[0178] S10, heating deionized water to 85° C., then adding nano-muscovite and stirring evenly to obtain a mixture, wherein the weight ratio of the nano-muscovite to water is 1:20;
[0179] S20, adjusting the pH of the mixture to 7.0-7.2 and continuing heating for 30 min, then adding octadecyl dimethyl benzyl ammonium chloride and stirring evenly (the weight ratio of the octadecyl dimethyl benzyl ammonium chloride to the nano muscovite is 1:10), and adjusting the pH value to 7.0-7.2, reacting for 2 h, filtering the obtained reaction solution, washing the filtered solid with deionized water for 3 times, and then drying at 80 ° C for 48 h, and finally grinding and sieving to obtain modified nano muscovite.
[0180] Example 7
[0181] This embodiment is used to illustrate the composite tube of the present invention.
[0182] The composite pipe comprises an inner lining layer 1, a reinforcement layer 2 and an outer pipe 3 arranged in sequence from the inside to the outside;
[0183] The inner lining layer is prepared by the method for preparing the inner lining layer described in Example 1;
[0184] The reinforcement layer is made of a continuous fiber reinforced resin prepreg tape, wherein the continuous fiber in the continuous fiber reinforced resin prepreg tape is glass fiber, and the resin matrix is high-density polyethylene. The preparation method of the reinforcement layer comprises: heating a continuous glass fiber reinforced prepreg tape with a width of 40 mm by radiation, and cross-winding the prepreg tape at an angle of 55° with the axis of the inner liner layer on the outer side of the inner liner layer, and the number of winding layers is 10;
[0185] The outer tube contains an anti-ultraviolet agent (poly{[6-[(1,1,3,3-tetramethylbutyl)amino]]-1,3,5-triazine-2,4-[(2,2,6,6,-tetramethyl-piperidinyl)imine), a plasticizer (polyolefin elastomer POE), a flame retardant (diethylaluminum hypophosphite), an antioxidant (pentaerythritol tetrakis(3,5-di-tert-butyl-4-hydroxy)phenylpropionate) and a medium-density polyethylene (brand name SP988, melt index 0.6g / 10min), the preparation method of the outer tube comprises: adding 1wt% of anti-ultraviolet agent, 1wt% of plasticizer, 1wt% of flame retardant, 1wt% of antioxidant and 96wt% of medium-density polyethylene into a high-speed mixing barrel of an extruder according to mass percentage for mixing, heating the obtained outer tube material particles for injection molding and placing them in a vacuum cavity, and then cooling and shaping and demolding to obtain an outer tube coated on the outside of the reinforcement layer, and the wall thickness of the outer tube is 3mm and the outer diameter is 88mm.
[0186] Embodiments 8 to 12
[0187] The method described in Example 7 is used for implementation, except that the lining layer in Example 8 is prepared by the method described in Example 2, the lining layer in Example 9 is prepared by the method described in Example 3, the lining layer in Example 10 is prepared by the method described in Example 4, the lining layer in Example 11 is prepared by the method described in Example 5, and the lining layer in Example 12 is prepared by the method described in Example 6.
[0188] Comparative Example 1
[0189] The method described in Example 1 was followed, except that the first auxiliary agent was not added (the first auxiliary agent was replaced by an equal amount of high-density polyethylene b);
[0190] Specifically, step A11 is: weighing the raw material components according to the following weight percentages: 88 wt% of high-density polyethylene b, 2 wt% of modified nanofiller and 10 wt% of antibacterial agent.
[0191] Comparative Example 2
[0192] The method described in Example 1 was followed, except that the nano-montmorillonite was not modified;
[0193] Specifically, step A11 is: weighing the raw material components according to the following weight percentages: 87 wt% of high-density polyethylene b, 2 wt% of nano-montmorillonite, 10 wt% of the antibacterial agent and 1 wt% of the first auxiliary agent.
[0194] Comparative Example 3
[0195] The method described in Example 1 is followed, except that the antibacterial barrier material is not prepared first. Specifically, all raw materials are directly mixed and co-extruded using the method of step A22.
[0196] Comparative Example 4
[0197] The method described in Example 1 was followed, except that when preparing the antibacterial barrier material, the content of the modified nanofiller was 8 wt %;
[0198] Specifically, step A11 is: weighing the raw material components according to the following weight percentages: 81 wt% of high-density polyethylene b, 8 wt% of modified nanofiller, 10 wt% of antibacterial agent and 1 wt% of the first auxiliary agent.
[0199] Comparative Example 5
[0200] The method described in Example 1 was followed, except that no antimicrobial barrier material was added when preparing the inner lining layer;
[0201] Specifically, the preparation method of the inner liner includes: A21, weighing the raw material components according to the following weight percentages: 99wt% of high-density polyethylene a and 1wt% of the second auxiliary agent;
[0202] A22. Add high-density polyethylene a and the second auxiliary agent into a twin-screw extruder and mix them evenly. In the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C. The head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C. After the material is extruded from the twin-screw extruder, it is cooled and shaped to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0203] Comparative Example 6
[0204] The method described in Example 1 was used to prepare the inner lining layer.
[0205] Specifically, the preparation method of the lining layer includes: adding high-density polyethylene a into a twin-screw extruder and mixing evenly, in the twin-screw extruder, the body temperature includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone one is 120°C, the temperature of zone two is 150°C, and the temperature of zone three is 190°C, the head temperature includes the neck temperature and the die temperature, wherein the neck temperature is 180°C, and the die temperature is 170°C, and the material is cooled and shaped after being extruded from the twin-screw extruder to obtain an inner lining layer with a wall thickness of 5 mm and an inner diameter of 65 mm.
[0206] Comparative Example 7
[0207] The method of Example 7 is used for implementation, except that the inner lining layer of the composite pipe is prepared by the method described in Comparative Example 6.
[0208] Test Example 1
[0209] The inner lining layer sample prepared in Example 1 was cut into small pieces of about 5 g, put into a flat vulcanizer, and the tableting temperature was 150°C, the pressure was 10 MPa, the time was 3 min, and air-cooled. After cutting, an antibacterial high barrier film sample of 50 mm × 50 mm × 0.2 mm was obtained; then the inner lining layers in Examples 2-6 and Comparative Examples 1-6 were also made into film samples according to the same method, and the following tests were performed respectively.
[0210] (1) The film samples obtained in Example 1 and Comparative Example 6 (pure HDPE) were characterized using a scanning electron microscope. The results are as follows: Figure 2 (Comparative Example 6) and Figure 3 (Example 1) shown.
[0211] Depend on Figure 2 and Figure 3 It can be seen that in the inner liner prepared in Example 1, the modified nano-montmorillonite and the antibacterial agent are uniformly dispersed in the HDPE, and the HDPE matrix tightly wraps the modified nano-montmorillonite and the antibacterial agent particles without holes.
[0212] (2) The helium permeability of the film samples prepared in Examples 1-6 and Comparative Examples 1-6 was tested by a gas permeometer (the gases contained in medium and high pressure oil and gas are usually oxygen, carbon dioxide, methane, hydrogen sulfide, etc., and the diameter and volume of helium are smaller than those of these gas molecules). The results are shown in Table 1.
[0213] Table 1
[0214] project <![CDATA[Permeability coefficient (cm 3 ·cm) / (cm 2 ·s·Pa)]]> Example 1 <![CDATA[2.94×10 -15 ]]> Example 2 <![CDATA[3.21×10 -15 ]]> Example 3 <![CDATA[4.85×10 -15 ]]> Example 4 <![CDATA[5.05×10 -15 <!-- 13 -->]]> Example 5 <![CDATA[4.41×10 -15 ]]> Example 6 <![CDATA[7.13×10 -15 ]]> Comparative Example 1 <![CDATA[9.35×10 -14 ]]> Comparative Example 2 <![CDATA[2.27×10 -13 ]]> Comparative Example 3 Membrane rupture Comparative Example 4 <![CDATA[1.35×10 -13 ]]> Comparative Example 5 <![CDATA[3.24×10 -13 ]]> Comparative Example 6 <![CDATA[2.24×10 -13 ]]>
[0215] It can be seen from Table 1 that the inner lining sample made of the inner lining material of the present invention has a very low permeability coefficient and has good gas barrier properties.
[0216] It can be seen from Example 1 and Example 5 that the addition of the second auxiliary agent has little effect on the gas barrier properties of the liner layer.
[0217] It can be seen from Example 1 and Example 6 that the effect of nano-montmorillonite is better.
[0218] It can be seen from Example 1 and Comparative Example 1 that the gas barrier property of the liner layer can be improved by adding the first auxiliary agent.
[0219] It can be seen from Example 1 and Comparative Example 2 that the gas barrier properties of the lining layer can be greatly improved by modifying the flaky nanofiller. It is speculated that this may be because the unmodified flaky nanofiller has poor dispersibility in high-density polyethylene, resulting in its gas barrier properties being very little changed compared to the lining layer made without adding antibacterial barrier material (i.e., Comparative Examples 5-6).
[0220] The film of Comparative Example 3 broke during the permeation test. This may be because it is difficult to evenly disperse the nanofillers, antimicrobial agents, etc. in the high-density polyethylene by direct mixing. The nanofillers and antimicrobial agents agglomerate, and holes appear in the test film, causing the permeability test to fail.
[0221] It can be seen from Example 1 and Comparative Example 4 that when preparing the antibacterial barrier material, the added amount of the modified nanofiller is not necessarily the better, but the gas barrier property is better when it is 2-6%.
[0222] It can be seen from Example 1 and Comparative Examples 5-6 that the gas barrier property of the lining layer can be greatly improved by adding the antibacterial barrier material.
[0223] It can be seen from Comparative Examples 5 and 6 that, although the addition of the second auxiliary agent improves the processing performance and antioxidant properties of the material, it has a certain adverse effect on the permeability of the material.
[0224] (3) The film samples prepared in Example 1 and Comparative Examples 1-6 were subjected to antibacterial tests according to the antibacterial test standard QB / T2591-2003A "Test methods and antibacterial effects of antibacterial plastics". The test bacteria were sulfate-reducing bacteria. The test results are shown in Table 2.
[0225] Table 2
[0226]
[0227]
[0228] It can be seen from Table 2 that the antibacterial rate of the lining layer sample made of the lining layer material provided by the present invention reaches 99%, and the antibacterial performance is excellent.
[0229] Test Example 2
[0230] The DN65 composite pipes prepared in Example 7 (the inner lining provided in Example 1) and Comparative Example 7 (the inner lining provided in Comparative Example 6) were cut into 10 cm long sections as interlayer bonding strength samples of the composite pipes. The samples were placed in a universal testing machine, and pressure was gradually applied to the inner lining to measure the displacement changes of the reinforcing layer and the inner lining during the shearing process. The results are shown in FIG. Figure 4 and Figure 5 As shown in the figure, the sample material shows yielding phenomenon, and it is believed that the lining layer of the composite pipe and the reinforcement layer begin to peel off; when the load applied by the testing machine reaches the maximum value and remains unchanged, or even slightly decreases, the lining layer of the composite pipe has peeled off from the reinforcement layer. Then, the interlayer bonding force of the pipeline is calculated according to the following formula as shown in Table 3, where D refers to the pipe diameter, L refers to the length of the pipe section, and W refers to the load applied by the testing machine on the pipeline.
[0231]
[0232] Table 3
[0233] project Bonding strength (MPa) Example 7 3.13 Comparative Example 7 2.5
[0234] It can be seen from Table 3 that the composite tube prepared by Example 7 has an obvious elastic deformation stage in the test, and the interlayer bonding strength is significantly greater than that of the composite tube prepared by Comparative Example 7, indicating that the lining material provided by the present invention improves the anti-interlayer delamination property of the lining layer prepared by the addition of antibacterial barrier material, so that it has good bonding with the reinforcement layer.
[0235] Since the principles of preparing the inner lining layer in Examples 2 to 6 are similar to those in Example 1, they also have good antibacterial properties and resistance to interlayer delamination.
[0236] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A lining material, It is characterized in that The inner lining material contains high-density polyethylene a and antibacterial barrier material, The antibacterial barrier material contains high-density polyethylene b, modified nanofiller, antibacterial agent and a first auxiliary agent, wherein the modified nanofiller is obtained by modifying a sheet-like nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer; Based on the total weight of the antibacterial barrier material, the content of the modified nano filler is 2-6wt%.
2. The lining material according to claim 1, It is characterized in that Based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%; Preferably, the flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite; Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.
3. The lining material according to claim 1 or 2, It is characterized in that The modified nanofiller is prepared according to the following process: S10, heating water to 70-90° C., and then mixing the water with the flaky nanofiller to obtain a mixture; S20, adjusting the pH of the mixture to 6.8-7.5 and continuing heating for 30-50 minutes, then reacting with a cationic surfactant, separating the obtained reaction liquid into solid and liquid, and then washing, drying, grinding and sieving the obtained solid.
4. The lining material according to claim 3, It is characterized in that In step S10, the weight ratio of the flaky nanofiller to water is 1:25-50; Preferably, the weight ratio of the cationic surfactant to the flaky nanofiller is 1:10-20.
5. The lining material according to claim 1 or 2, It is characterized in that The melt index of the high-density polyethylene b is 0.3 to 0.5 g / 10 min; Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide; Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer; Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
6. The lining material according to claim 1, It is characterized in that The antibacterial barrier material is prepared according to the following process: high-density polyethylene, modified nanofiller, antibacterial agent and first auxiliary agent are blended and extruded; Preferably, the blending extrusion is carried out in a twin-screw extruder; Preferably, the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
7. The lining material according to claim 1, It is characterized in that Based on the total weight of the inner lining material, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%; Preferably, the high-density polyethylene a and the high-density polyethylene b are the same; Preferably, the inner lining material further contains a second auxiliary agent, and the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent; Preferably, in the inner lining material, the content of the second auxiliary agent is 1-2 wt %.
8. A method for preparing an inner lining layer, It is characterized in that The method includes: A1, blending and extruding high-density polyethylene b, modified nanofiller, antibacterial agent and first auxiliary agent, cooling and granulating to obtain antibacterial barrier material; A2, blending and extruding the antibacterial barrier material and high-density polyethylene a; Wherein, in step A1, the modified nanofiller is obtained by modifying a flaky nanofiller with a cationic surfactant, and the first auxiliary agent is a coupling agent and / or a compatibilizer.
9. The method according to claim 8, It is characterized in that In step A1, based on the total weight of the antibacterial barrier material, the content of the high-density polyethylene b is 79-90wt%, the content of the modified nanofiller is 2-6wt%, the content of the antibacterial agent is 4-10wt%, and the content of the first auxiliary agent is 1-5wt%; Preferably, in step A1, the blending extrusion is carried out in a twin-screw extruder, wherein the working temperature of the twin-screw extruder is 160-200° C., the working speed is 300-350 r / min, and the working time is 3-6 min.
10. The method according to claim 8 or 9, It is characterized in that The flaky nanofiller is selected from one or more of muscovite, biotite, phlogopite, kaolin and montmorillonite; Preferably, the cationic surfactant is a long-chain alkyl quaternary ammonium salt, preferably one or more of dodecyltrimethylammonium chloride, hexadecyltrimethylammonium bromide, hexadecyltrimethylammonium chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride; Preferably, the melt index of the high-density polyethylene b is 0.3 to 0.5 g / 10 min; Preferably, the antibacterial agent is nano copper oxide and / or nano silver oxide; Preferably, the compatibilizer is selected from one or more of maleic anhydride grafted high-density ethylene, maleic anhydride grafted ethylene-1-octene block copolymer, acrylic acid grafted polyethylene and maleic anhydride grafted ethylene-vinyl acetate copolymer; Preferably, the coupling agent is a silane coupling agent and / or a titanate coupling agent.
11. The method according to claim 8 or 9, It is characterized in that The method also includes preparing the modified nanofiller according to the following steps: The water is heated to 70-90° C., and then mixed with the flaky nanofiller to obtain a mixture; The pH of the mixture is adjusted to 6.8-7.5 and continued to be heated for 30-50 minutes, and then reacted with a cationic surfactant, the obtained reaction liquid is separated into solid and liquid, and then the obtained solid is washed, dried, ground and sieved.
12. The method according to claim 8, It is characterized in that In step A2, the blending extrusion is carried out in a twin-screw extruder; Preferably, in step A2, the body temperature of the twin-screw extruder includes three temperature zones arranged in sequence along the material flow direction, the temperature of zone 1 is 110-130° C., the temperature of zone 2 is 140-160° C., and the temperature of zone 3 is 180-200° C.; Preferably, in step A2, the head temperature of the twin-screw extruder is 165-185°C.
13. The method according to any one of claims 8 to 12, It is characterized in that In step A2, based on the total weight of the antibacterial barrier material and the high-density polyethylene a, the content of the high-density polyethylene a is 80-95wt%, and the content of the antibacterial barrier material is 5-20wt%; Preferably, the high-density polyethylene a and the high-density polyethylene b are the same; Preferably, step A2 comprises: blending and extruding the antibacterial barrier material, high-density polyethylene a and a second auxiliary agent, wherein the second auxiliary agent is selected from one or more of a plasticizer, an antioxidant and an anti-ultraviolet agent; Preferably, in step A2, based on the total weight of the high-density polyethylene a, the antibacterial barrier material and the second auxiliary agent, the content of the second auxiliary agent is 1-2 wt %.
14. A composite pipe, It is characterized in that The composite pipe comprises an inner lining layer, a reinforcement layer and an outer pipe arranged in sequence from the inside to the outside; The inner lining layer is made of the inner lining layer material described in any one of claims 1-7 or is made of the method described in any one of claims 8-13.
15. The composite pipe according to claim 14, It is characterized in that The reinforcement layer is made of continuous fiber reinforced resin prepreg tapes wound around the outer side of the inner lining layer in a cross manner; Preferably, the outer tube is made of a raw material containing medium-density polyethylene or low-density polyethylene.
16. The composite pipe according to claim 14, It is characterized in that The melt index of the medium-density polyethylene or low-density polyethylene is 0.5 to 0.7 g / 10 min; Preferably, the raw material for preparing the outer tube further contains a third auxiliary agent, wherein the third auxiliary agent is selected from one or more of a plasticizer, a flame retardant, an antioxidant, a masterbatch and an anti-ultraviolet agent.
Citation Information
Patent Citations
Polymer composite material with high gas barrier property
CN114456470A
Pipe having barrier property
CN101072822A
Composite pipe with distributed barrier properties
RU204545U1
Pipe having barrier property
US20060121227A1
Cited By
Preparation method of antibacterial wear-resistant PE water supply pipe
CN119859336A