Environment-friendly antibacterial color master batch and preparation method thereof
By using modified silver cerium zinc-doped silica and cyclodextrin modified natural antibacterial agents in masterbatches, combined with degradable modified polyethylene resin and modified pigments, the antibacterial properties and environmental protection of traditional masterbatches are solved. The problem of insufficient properties has achieved the improvement of the excellent antibacterial properties, degradability and mechanical properties of the masterbatch, and met the market's demand for environmentally friendly antibacterial masterbatch.
Patent Information
- Application Number
- CN202410967472.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional masterbatches have shortcomings in antibacterial performance and environmental protection, and it is difficult to meet the market's demand for environmentally friendly and antibacterial functions.
Modified silver cerium zinc-doped silica and cyclodextrin modified natural antibacterial agents are used as composite antibacterial agents, combined with degradable modified polyethylene resin and modified pigment, and the antibacterial performance of masterbatches is improved through modification treatment. Mechanical properties and degradability.
It has achieved the improvement of excellent antibacterial properties, degradability and mechanical properties of masterbatches, and its performance is long-term and stable, and it complies with green environmental protection standards.
Smart Images

Figure BDA0004952175360000091
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of masterbatch preparation, and in particular to an environmentally friendly antibacterial masterbatch and a preparation method thereof. Background Art
[0002] Polyethylene is a thermoplastic resin made from the polymerization reaction of ethylene monomer. It is the most widely used general-purpose plastic in the world because of its good comprehensive properties, non-toxicity, easy molding and processing, and low price. It is widely used in packaging materials, daily necessities, office supplies, medical supplies, gas transmission, water supply, sewage discharge, agricultural irrigation, as well as oil fields, chemicals, mining, post and telecommunications.
[0003] Masterbatches are widely used in the production of various plastic products as plastic colorants. However, traditional masterbatches often only focus on coloring effects and ignore environmental protection and antibacterial properties. As consumers pay more and more attention to product safety and environmental protection, the market is in urgent need of a masterbatch that is both environmentally friendly and has antibacterial functions. At present, although some products try to add antibacterial agents to improve antibacterial properties, it is often difficult to achieve the ideal antibacterial effect, or the masterbatch cannot be effectively degraded, does not meet environmental protection standards, and cannot meet the increasingly stringent market demand. Summary of the invention
[0004] In view of the shortcomings of the prior art, the present application provides an environmentally friendly antibacterial masterbatch and a preparation method thereof. The environmentally friendly antibacterial masterbatch of the present application has excellent antibacterial properties, degradability and mechanical properties, and has long-term stable performance, and has important application value in the field of polyethylene masterbatch technology.
[0005] In the first aspect, the present application provides an environmentally friendly antibacterial masterbatch, which adopts the following technical solution: An environmentally friendly antibacterial masterbatch, wherein the raw materials for preparation include, by weight: 30-35 parts of linear low-density polyethylene, 25-28 parts of degradable modified polyethylene resin, 28-32 parts of modified pigment, 0.1-0.3 parts of antioxidant, 3-4 parts of polyethylene wax, 0.5-0.8 parts of composite antibacterial agent, and 1-2 parts of coupling agent, wherein the composite antibacterial agent is composed of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent.
[0006] By adopting the above technical scheme, the environmentally friendly antibacterial masterbatch of the present application has excellent antibacterial performance, degradability and mechanical properties, and the performance is long-term and stable, and has important application value in the field of polyethylene masterbatch technology. Among them, linear low-density polyethylene and degradable modified polyethylene resin are the main raw materials for preparing environmentally friendly antibacterial masterbatch. They have good compatibility and can effectively improve the mechanical properties and degradability of masterbatch; modified pigments can improve the color stability of masterbatch; antioxidants can prevent masterbatch from deteriorating due to oxidation during use; polyethylene wax can improve the processing performance and surface finish of masterbatch; composite antibacterial agent can give masterbatch excellent antibacterial performance; coupling agent can improve the binding force between the components in masterbatch.
[0007] Preferably, the mass ratio of the modified silver-cerium-zinc doped silica to the cyclodextrin modified natural antibacterial agent is 5:3-5.
[0008] By adopting the above technical scheme, firstly, the modified silver-cerium-zinc doped silica is modified by vinyl triethoxysilane, which greatly improves its compatibility with linear low-density polyethylene and degradable modified polyethylene resin and its own dispersibility. This enables the modified silver-cerium-zinc doped silica to be better dispersed in the polyethylene resin matrix, thereby significantly improving the antibacterial and mechanical properties of the environmentally friendly antibacterial masterbatch. Secondly, cyclodextrin-modified natural antibacterial agents (such as purslane powder) have good antibacterial properties and are non-toxic to human skin, meeting the requirements of the green environmental protection era. Through cyclodextrin coating, the shortcomings of purslane powder that it is not resistant to high temperatures, as well as the compatibility and dispersibility problems, are overcome. At the same time, the cyclodextrin-modified natural antibacterial agent and the modified silver-cerium-zinc doped silica work synergistically, further improving the antibacterial and mechanical properties of the environmentally friendly antibacterial masterbatch. In summary, the mass ratio of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent of 5:3-5 played a synergistic role in the present application, and jointly improved the antibacterial and mechanical properties of the environmentally friendly antibacterial masterbatch.
[0009] Preferably, the preparation method of the modified silver-cerium-zinc doped silica comprises the following steps: S31, at room temperature, add 300 mL of tetra-n-butyl silicate to 400 mL of ethanol and stir for 40 min to form solution A; S32, adding 0.7 g of silver nitrate, 8 g of cerium nitrate and 15 g of zinc nitrate to a solution consisting of 300 mL of ethanol, 18 mL of acetic acid and 120 mL of water to form solution B; S33, adding solution B dropwise into solution A, stirring for 40 min, heating to 43° C., standing for 12 h, then centrifuging, washing, drying at 92° C. for 15 h, and finally calcining at 530° C. for 3 h, cooling, and grinding to obtain silver-cerium-zinc-doped silica; S34, mixing 0.8 g of vinyl triethoxysilane with 60 g of ethanol and 40 g of water, stirring evenly to obtain a mixture C; S35. Add the obtained silver-cerium-zinc doped silica to mixture C, then heat it to 40°C, stir it at 200 r / min for 150 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-zinc doped silica, wherein the particle size of the modified silver-cerium-zinc doped silica is 30-50 nm.
[0010] By adopting the above technical scheme, the effect of the prepared modified silver-cerium-zinc doped silica is mainly reflected in the following aspects: the modified silver-cerium-zinc doped silica has excellent antibacterial properties and can effectively inhibit the growth and reproduction of bacteria. The antibacterial properties of the environmentally friendly antibacterial masterbatch are further improved by synergistic action with the cyclodextrin modified natural antibacterial agent. The modified silver-cerium-zinc doped silica has good compatibility and dispersibility with linear low-density polyethylene and degradable modified polyethylene resin, which helps to improve the mechanical properties of the environmentally friendly antibacterial masterbatch. The modified silver-cerium-zinc doped silica synergizes with the cyclodextrin modified natural antibacterial agent to improve the performance stability of the environmentally friendly antibacterial masterbatch, so that it maintains good antibacterial effects and mechanical properties during long-term use. The modified silver-cerium-zinc doped silica is an inorganic material, non-toxic and harmless, and meets the requirements of green environmental protection. At the same time, its degradability helps to reduce the impact of the product on the environment. By modifying silver-cerium-zinc doped silica with vinyl triethoxysilane, its compatibility and dispersibility with linear low-density polyethylene and degradable modified polyethylene resin are improved, which helps to improve the overall performance of environmentally friendly antibacterial masterbatch. In summary, the role and synergistic effect of modified silver-cerium-zinc doped silica in this application are mainly reflected in the improvement of antibacterial performance, mechanical properties, stability, environmental performance, compatibility and dispersibility.
[0011] Preferably, the preparation method of the cyclodextrin modified natural antibacterial agent is: 5 parts of cyclodextrin and 30 parts of purslane powder with a particle size of 5-8 microns are placed in a reactor according to their mass fractions, and then the temperature is raised to 40-50°C, and ultrasonically treated for 50-60 minutes at an ultrasonic power of 40 W to allow the cyclodextrin to fully coat the purslane powder to obtain the cyclodextrin modified natural antibacterial agent.
[0012] By adopting the above technical solution, the cyclodextrin modified natural antibacterial agent and the modified silver-cerium-zinc doped silica work together to improve the antibacterial properties of the environmentally friendly antibacterial masterbatch. Purslane powder is a natural antibacterial agent that is non-toxic to human skin and meets the requirements of the green environmental protection era. Through cyclodextrin coating, the shortcomings of purslane powder that it is not resistant to high temperatures, as well as its compatibility and dispersibility, are overcome. At the same time, it also works synergistically with the modified silver-cerium-zinc doped silica to improve the antibacterial properties and mechanical properties of the environmentally friendly antibacterial masterbatch.
[0013] Preferably, the method for preparing the degradable modified polyethylene resin comprises the following steps: S51. According to the mass fractions, 16.9 parts of 2-bromo-1,1-dimethoxyethane, 10.6 parts of 1,4-butanediol, 0.34 parts of p-toluenesulfonic acid and 45 parts of toluene were added into the reactor in sequence, the temperature was raised to 125°C, the mixture was stirred under reflux for 18-20 hours, and then washed with ethyl acetate for 3 times, and 2-bromo-1,3-dioxepane was obtained by vacuum distillation. Then 33 parts of tetrahydrofuran and 14.1 parts of potassium tert-butoxide were added, the mixture was stirred for 80-85 minutes, the temperature was lowered to room temperature, the reaction was continued with stirring for 14 hours, ether was added, the mixture was filtered, the mixture was washed with ether and filtered, and the filtrate was vacuum distilled to obtain an intermediate; S51. According to the mass proportions, 20.5 parts of the intermediate, 13.9 parts of N-vinylcaprolactam and 68.8 parts of toluene are added into the reactor, and then 8.34 parts of thiourea chitosan-Co (Ⅱ) complex and 0.28 parts of azobisisobutyronitrile are added. Ethylene is introduced under nitrogen protection at a pressure of 29 bar. The temperature is raised to 75°C, and the mixture is stirred and reacted for 24 hours. The solvent is removed by distillation under reduced pressure, and the filter cake is filtered. After washing three times with toluene, the filter cake is dried at 72°C for 24 hours to obtain a crude product. The crude product is pulverized and passed through a 100-mesh sieve to obtain a degradable modified polyethylene resin.
[0014] By adopting the above technical scheme, toluene is used as a solvent in the preparation of degradable modified polyethylene resin, and a small part of it will participate in the reaction or remain after distillation, so that the degradable modified polyethylene has a slight aromatic smell; the molecular chain contains a hydrophilic and easily degradable caprolactam structure, and the introduction of thiourea chitosan-Co (Ⅱ) complex improves the reaction activity and strength, facilitates processing and molding, and increases the degradation rate of environmentally friendly antibacterial masterbatch. The role of degradable modified polyethylene resin is to provide excellent mechanical properties and degradability, and synergize with linear low-density polyethylene to improve the overall performance of environmentally friendly antibacterial masterbatch.
[0015] Preferably, the method for preparing the modified pigment comprises the following steps: S61. According to the mass fractions, 10 parts of pigment and 3 parts of dimer acid polyester polyol were added to 20 parts of toluene, and ultrasonic dispersion was performed for 30 minutes. Then 6 parts of toluene-2,4-diisocyanate and 0.03 parts of dibutyltin dilaurate were added, and mechanical stirring was performed to mix well. The system was transferred to a reactor at 63°C and reacted for 10 hours. After the reaction, the system was filtered, washed and dried to obtain an isocyanate-activated pigment. S62. According to the mass fractions, 10 parts of isocyanate-activated pigment were added to 25 parts of N,N-dimethylformamide, and ultrasonic dispersion was performed for 30 minutes. Then 15 parts of hydroxyl-terminated polysiloxane and 0.01 parts of dibutyltin dilaurate were added, and the mixture was stirred well. Then the system was transferred to a reactor at 80°C and reacted for 3 hours. After the reaction, the system was filtered, and the filter cake was washed with ethanol and vacuum dried to obtain a modified pigment.
[0016] By adopting the above technical scheme, the role of the modified pigment is to improve the interfacial affinity between the pigment and the polyethylene resin, making it easier to disperse in the polyethylene resin matrix, avoiding the negative impact caused by the agglomeration problem. By chemically bonding the hydroxyl-terminated polysiloxane to the pigment surface, the surface modification of the pigment is achieved. Since the hydroxyl-terminated polysiloxane structure contains a hydrophobic structure, after forming a chemical connection with the pigment, the hydrophilic and oleophobic properties of the pigment surface can be effectively changed. In addition, the modified pigment also synergizes with the modified silver-cerium-zinc doped silica to improve the mechanical properties of the environmentally friendly antibacterial masterbatch. These synergistic effects make the environmentally friendly antibacterial masterbatch of the present application have excellent antibacterial properties, degradability and mechanical properties, and the performance is long-term and stable, and has important application value in the field of polyethylene masterbatch technology.
[0017] Preferably, the pigment is one of titanium dioxide, red iron oxide and yellow iron oxide.
[0018] Preferably, the antioxidant is at least one of antioxidant 1010, antioxidant 1076 and antioxidant 168.
[0019] Preferably, the coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyloxypropyl trimethoxysilane in a mass ratio of 3:4:3.
[0020] By adopting the above technical scheme, the role of these three coupling agents in the environmentally friendly antibacterial masterbatch is mainly to improve the interfacial compatibility between the inorganic filler and the organic resin, enhance the interaction between the two, and thus improve the mechanical properties and antibacterial properties of the material. Vinyl triethoxysilane is a commonly used silane coupling agent, which can generate silanols through hydrolysis reaction, and then undergo condensation reaction with the hydroxyl groups on the surface of the inorganic filler to form a stable chemical bond. At the same time, the vinyl group of vinyl triethoxysilane can react with polyethylene resin by free radicals, thereby realizing the chemical connection between the inorganic filler and the polyethylene resin. This connection method can significantly improve the dispersibility and compatibility of the inorganic filler in the polyethylene resin, thereby improving the mechanical properties and antibacterial properties of the material. γ-mercaptopropyl trimethoxysilane is a silane coupling agent containing a mercapto group, and its mercapto group can react with the silver ions in the silver-cerium-zinc doped silica to form a stable complex. This complex can improve the dispersibility and stability of the silver-cerium-zinc doped silica in the polyethylene resin, thereby enhancing the antibacterial properties of the material. At the same time, the methoxy group of γ-mercaptopropyl trimethoxysilane can undergo an ester exchange reaction with polyethylene resin to achieve a chemical connection between the inorganic filler and the polyethylene resin. γ-Glycidyloxypropyl trimethoxysilane is a silane coupling agent containing an epoxy group, and its epoxy group can undergo a ring-opening reaction with polyethylene resin to form a stable chemical bond. At the same time, the methoxy group of γ-Glycidyloxypropyl trimethoxysilane can undergo a condensation reaction with the hydroxyl group on the surface of the inorganic filler to achieve a chemical connection between the inorganic filler and the polyethylene resin. This connection method can improve the dispersibility and compatibility of the inorganic filler in the polyethylene resin, thereby improving the mechanical properties and antibacterial properties of the material. In summary, these three coupling agents have a synergistic effect in the environmentally friendly antibacterial masterbatch, jointly improving the interfacial compatibility between the inorganic filler and the polyethylene resin, and enhancing the interaction between the two, thereby improving the mechanical properties and antibacterial properties of the material.
[0021] In a second aspect, the present application provides a method for preparing an environmentally friendly antibacterial masterbatch, using the following technical solution: As a general technical concept, the present application also provides a method for preparing the above-mentioned environmentally friendly antibacterial masterbatch, wherein linear low-density polyethylene, degradable modified polyethylene resin, modified pigment, antioxidant, polyethylene wax, composite antibacterial agent and coupling agent are sequentially added into an internal mixer for internal mixing, the internal mixing temperature is 130°C, and the internal mixing time is 10-20min; after discharging, the material mass is added into a twin-screw extruder through a feeder for extrusion granulation, the extrusion temperature is 190-230°C, and the screw speed is 280-350rpm, to obtain an environmentally friendly antibacterial masterbatch.
[0022] In summary, the present application includes at least one of the following beneficial technical effects: 1. Excellent antibacterial properties: Through the synergistic effect of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agents, as well as the introduction of purslane powder, the masterbatch has excellent antibacterial properties, which can effectively inhibit the growth and reproduction of bacteria and improve the hygiene and safety of the product.
[0023] 2. Degradability: Degradable modified polyethylene resin is used as one of the raw materials. Its molecular chain contains hydrophilic and easily degradable caprolactam structure. At the same time, the introduction of thiourea chitosan-Co (Ⅱ) complex improves the reaction activity and strength, making the masterbatch have good degradability, which is beneficial to reduce environmental pollution.
[0024] 3. Good mechanical properties: By improving the compatibility of modified silver-cerium-zinc-doped silica with linear low-density polyethylene and degradable modified polyethylene resin, as well as improving its own dispersibility, and the surface modification of the pigment improves the interfacial affinity between the pigment and the polyethylene resin, the masterbatch has good mechanical properties and can meet the application needs of different fields.
[0025] 4. Long-term stable properties: Due to the synergistic effect of multiple modifiers and antibacterial agents, as well as the optimized preparation process, the performance of the masterbatch is long-term stable, not easy to fail or deteriorate, and the service life of the product is extended.
[0026] 5. Green and environmentally friendly: The environmentally friendly antibacterial masterbatch of this application meets the requirements of the green and environmentally friendly era, does not contain substances harmful to the human body, and does not pollute the environment during production and use. DETAILED DESCRIPTION
[0027] The following will describe the implementation scheme of the present application in detail with reference to the examples, but those skilled in the art will understand that the following examples are only used to illustrate the present application and should not be considered to limit the scope of the present application. If the specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially, antioxidant 1010, tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid] pentaerythritol ester, purchased from BASF; antioxidant 1076, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionic acid n-octadecyl alcohol ester, purchased from BASF; antioxidant 168, tris(2,4-di-tert-butylphenyl) phosphite, purchased from BASF.
[0028] Preparation Example 1 Preparation of modified silver-cerium-zinc doped silica The preparation method of modified silver-cerium-zinc doped silicon dioxide comprises the following steps: S31, at room temperature, add 300 mL of tetra-n-butyl silicate to 400 mL of ethanol and stir for 40 min to form solution A; S32, adding 0.7 g of silver nitrate, 8 g of cerium nitrate and 15 g of zinc nitrate to a solution consisting of 300 mL of ethanol, 18 mL of acetic acid and 120 mL of water to form solution B; S33, adding solution B dropwise into solution A, stirring for 40 min, heating to 43° C., standing for 12 h, then centrifuging, washing, drying at 92° C. for 15 h, and finally calcining at 530° C. for 3 h, cooling, and grinding to obtain silver-cerium-zinc-doped silica; S34, mixing 0.8 g of vinyl triethoxysilane with 60 g of ethanol and 40 g of water, stirring evenly to obtain a mixture C; S35. Add the obtained silver-cerium-zinc doped silica to mixture C, then heat it to 40°C, stir it at 200 r / min for 150 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-zinc doped silica, wherein the particle size of the modified silver-cerium-zinc doped silica is 30-50 nm.
[0029] Preparation Example 2 Preparation of cyclodextrin modified natural antibacterial agent The preparation method of the cyclodextrin modified natural antibacterial agent is as follows: 50g of cyclodextrin and 300g of purslane powder with a particle size of 5-8 microns are put into a reactor according to the mass fractions, and then the temperature is raised to 45°C, and ultrasonic treatment is performed for 55 minutes at an ultrasonic power of 40W to allow the cyclodextrin to fully coat the purslane powder to obtain the cyclodextrin modified natural antibacterial agent.
[0030] Preparation Example 3 Preparation of degradable modified polyethylene resin The preparation method of the degradable modified polyethylene resin comprises the following steps: S51, according to the mass fraction, 16.9kg2-bromo-1,1-dimethoxyethane, 10.6kg1,4-butanediol, 0.34kgp-toluenesulfonic acid, 45kgtoluene were added into the reactor in sequence, the temperature was raised to 125°C, the mixture was stirred under reflux for 19h, the mixture was washed with ethyl acetate for 3 times, and 2-bromo-1,3-dioxepane was obtained by vacuum distillation, 33kgtetrahydrofuran and 14.1kgpotassium tert-butoxide were added, the mixture was stirred for 80-85min, the temperature was lowered to room temperature, the mixture was stirred for 14h, ether was added, the mixture was filtered, the mixture was washed with ether and filtered, and the filtrate was vacuum distilled to obtain an intermediate; S51. According to the mass proportions, 20.5 kg of the intermediate, 13.9 kg of N-vinyl caprolactam and 68.8 kg of toluene are added into the reactor, and then 8.34 kg of thiourea chitosan-Co (Ⅱ) complex and 0.28 kg of azobisisobutyronitrile are added. Ethylene is introduced under nitrogen protection at a pressure of 29 bar. The temperature is raised to 75°C, and the mixture is stirred and reacted for 24 hours. The solvent is removed by distillation under reduced pressure, and the filter cake is filtered. After washing three times with toluene, the filter cake is dried at 72°C for 24 hours to obtain a crude product. The crude product is pulverized and passed through a 100-mesh sieve to obtain a degradable modified polyethylene resin.
[0031] Preparation Example 4 Preparation of modified pigment The preparation method of the modified pigment comprises the following steps: S61. According to the mass fractions, 1.0 kg of pigment and 0.3 kg of dimer acid polyester polyol were added to 2.0 kg of toluene, and ultrasonic dispersion was performed for 30 min. 0.6 kg of toluene-2,4-diisocyanate and 0.003 kg of dibutyltin dilaurate were added, and mechanical stirring was performed to mix well. The system was transferred to a reactor at 63° C. and reacted for 10 h. After the reaction was completed, the system was filtered, washed, and dried to obtain an isocyanate-activated pigment, wherein the pigment was titanium dioxide; S62. According to the mass fractions, add 1.0 kg of isocyanate-activated pigment to 2.5 kg of N,N-dimethylformamide, ultrasonicate for 30 min, add 1.5 kg of hydroxyl-terminated polysiloxane and 0.001 kg of dibutyltin dilaurate, stir and mix evenly, transfer to a reactor at 80°C, react for 3 h, filter after the reaction is completed, wash the filter cake with ethanol, and vacuum dry to obtain a modified pigment.
[0032] Preparation Example 5 The same as Preparation Example 4, except that the pigment is iron oxide yellow.
[0033] Preparation Example 6 The same as Preparation Example 4, except that the pigment is red iron oxide.
[0034] Example 1 An environmentally friendly antibacterial masterbatch, the raw materials for preparation include: 30kg of linear low-density polyethylene, 25kg of degradable modified polyethylene resin, 28kg of modified pigment, 1010kg of antioxidant 0.1kg, 3kg of polyethylene wax, 0.5kg of composite antibacterial agent, and 1kg of coupling agent, wherein the composite antibacterial agent is composed of modified silver cerium zinc doped silica and cyclodextrin modified natural antibacterial agent in a mass ratio of 5:3, and the coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane in a mass ratio of 3:4:3; the modified pigment is prepared in Preparation Example 4; the above-mentioned method for preparing an environmentally friendly antibacterial masterbatch, linear low-density polyethylene, degradable modified polyethylene resin, modified pigment, antioxidant 1010, polyethylene wax, composite antibacterial agent and coupling agent are sequentially added into a mixer for mixing, the mixing temperature is 130°C, and the mixing time is 10min; after discharging, the material mass is added into a twin-screw extruder through a feeder for extrusion granulation, the extrusion temperature is 190°C, and the screw speed is 350rpm to obtain an environmentally friendly antibacterial masterbatch.
[0035] Example 2 An environmentally friendly antibacterial masterbatch, the raw materials for preparation include: 35kg of linear low-density polyethylene, 28kg of degradable modified polyethylene resin, 32kg of modified pigment, 1076kg of antioxidant 0.3kg, 4kg of polyethylene wax, 0.8kg of composite antibacterial agent, and 2kg of coupling agent, wherein the composite antibacterial agent is composed of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent in a mass ratio of 5:5, and the coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane in a mass ratio of 3:4:3; the modified pigment is prepared in Preparation Example 5; the preparation method of the above-mentioned environmentally friendly antibacterial masterbatch, linear low-density polyethylene, degradable modified polyethylene resin, modified pigment, antioxidant 1076, polyethylene wax, composite antibacterial agent and coupling agent are sequentially added into a mixer for mixing, the mixing temperature is 130°C, and the mixing time is 20min; after discharging, the material mass is added into a twin-screw extruder through a feeder for extrusion granulation, the extrusion temperature is 230°C, and the screw speed is 280rpm to obtain an environmentally friendly antibacterial masterbatch.
[0036] Example 3 An environmentally friendly antibacterial masterbatch, the raw materials for preparation include: 33kg of linear low-density polyethylene, 26kg of degradable modified polyethylene resin, 30kg of modified pigment, 168kg of antioxidant 0.2kg, 3.5kg of polyethylene wax, 0.6kg of composite antibacterial agent, and 1.5kg of coupling agent, wherein the composite antibacterial agent is composed of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent in a mass ratio of 5:4, and the coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyl ether oxypropyl trimethoxysilane in a mass ratio of 3:4:3; the modified pigment is prepared in Preparation Example 6; the above-mentioned method for preparing an environmentally friendly antibacterial masterbatch, linear low-density polyethylene, degradable modified polyethylene resin, modified pigment, antioxidant 168, polyethylene wax, composite antibacterial agent and coupling agent are sequentially added into a mixer for mixing, the mixing temperature is 130°C, and the mixing time is 15min; after discharging, the material mass is added into a twin-screw extruder through a feeder for extrusion granulation, the extrusion temperature is 210°C, and the screw speed is 300rpm to obtain an environmentally friendly antibacterial masterbatch.
[0037] Comparative Example 1 The same as Example 3, except that: the composite antibacterial agent is modified silver-cerium-zinc doped silica.
[0038] Comparative Example 2 The same as Example 3, except that the composite antibacterial agent is a cyclodextrin-modified natural antibacterial agent.
[0039] Comparative Example 3 The same as Example 3, except that: the coupling agent is vinyl triethoxy silane.
[0040] Comparative Example 4 The same as Example 3, except that: the coupling agent is γ-mercaptopropyltrimethoxysilane.
[0041] Comparative Example 5 The same as Example 3, except that: the coupling agent is γ-glycidyloxypropyltrimethoxysilane.
[0042] Comparative Example 6 The same as Example 3, except that an equal amount of linear low-density polyethylene is used instead of the degradable modified polyethylene resin.
[0043] Comparative Example 7 The same as Example 3, except that an equal amount of iron oxide red pigment is used instead of the modified pigment.
[0044] Performance testing The environmentally friendly antibacterial masterbatches prepared in Examples 1 to 3 and Comparative Examples 1 to 7 were sampled, respectively, and made into corresponding shapes according to different test standards, and the following performance tests were performed. The test results are shown in Table 1; Antibacterial property test: QB / T 2591-2003A "Test methods and antibacterial effects of antibacterial plastics" was used to test the antibacterial properties during preparation and after 30 days of storage; Tensile strength and elongation at break test: According to GB / T 1040-2006, the tensile strength and elongation at break of the specimens were tested using a DL-JYDZ8300T tensile strength tester; Degradation rate test: The soil burial method is used. The obtained products are dried and buried in moist soil. The temperature during the experiment is maintained at 25-30°C. After 90 days, the samples are taken out of the soil, washed, dried, weighed, and the sample weight loss rate is calculated.
[0045] Table 1 Performance test Analyzing the data in Table 1, we can see that: 1) The environmentally friendly antibacterial masterbatches prepared in Examples 1 to 3 have excellent antibacterial properties, degradability and mechanical properties, and the properties are long-lasting and stable, and have important application value in the field of polyethylene masterbatch technology.
[0046] 2) The comparative analysis of the performance of the environmentally friendly antibacterial masterbatch prepared in combination with Example 3 and Comparative Examples 1-2 shows that the mass ratio of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent is 5:4, and the synergistic effect between them is utilized to further improve the antibacterial performance and mechanical properties of the environmentally friendly antibacterial masterbatch.
[0047] 3) The performance comparison analysis of the environmentally friendly antibacterial masterbatch prepared in combination with Example 3 and Comparative Examples 3 to 5 shows that the coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyloxypropyl trimethoxysilane in a mass ratio of 3:4:3. The synergistic effect between them is utilized to jointly improve the interfacial compatibility between the inorganic pigment and the polyethylene resin, enhance the interaction between the two, thereby improving the mechanical properties and antibacterial properties of the material.
[0048] 4) The comparative analysis of the performance of the environmentally friendly antibacterial masterbatch prepared in combination with Example 3 and Comparative Example 6 shows that the role of the degradable modified polyethylene resin is to provide excellent mechanical properties and degradability, and to synergize with the linear low-density polyethylene to improve the overall performance of the environmentally friendly antibacterial masterbatch.
[0049] 5) The performance comparison analysis of the environmentally friendly antibacterial masterbatch prepared in combination with Example 3 and Comparative Example 7 shows that the role of the modified pigment is to improve the interfacial affinity between the pigment and the polyethylene resin, making it easier to disperse in the polyethylene resin matrix, avoiding the negative impact caused by the agglomeration problem. The surface modification of the pigment is achieved by chemically bonding the hydroxyl-terminated polysiloxane to the pigment surface. Since the hydroxyl-terminated polysiloxane structure contains a hydrophobic structure, after forming a chemical connection with the pigment, the hydrophilic and oleophobic properties of the pigment surface can be effectively changed. In addition, the modified pigment also synergizes with the modified silver-cerium-zinc-doped silica to enhance the mechanical properties and antibacterial properties of the environmentally friendly antibacterial masterbatch. These synergistic effects make the environmentally friendly antibacterial masterbatch of the present application have excellent antibacterial properties, degradability and mechanical properties, and the performance is long-term and stable, and has important application value in the field of polyethylene masterbatch technology.
[0050] The above embodiments are only used to explain the technical solutions of the present application rather than to limit them. Although the above embodiments provide a specific description of the present application, relevant technical personnel should understand that the specific implementation methods of the present application can still be modified or replaced by equivalents, and any modifications and equivalent replacements that do not depart from the spirit and scope of the present application should be included in the protection scope of the present application.
Claims
1. An environmentally friendly antibacterial masterbatch, characterized in that: The raw materials for preparation include, by weight: 30-35 parts of linear low-density polyethylene, 25-28 parts of degradable modified polyethylene resin, 28-32 parts of modified pigment, 0.1-0.3 parts of antioxidant, 3-4 parts of polyethylene wax, 0.5-0.8 parts of composite antibacterial agent, and 1-2 parts of coupling agent, wherein the composite antibacterial agent is composed of modified silver-cerium-zinc doped silica and cyclodextrin modified natural antibacterial agent.
2. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The mass ratio of the modified silver-cerium-zinc doped silica to the cyclodextrin modified natural antibacterial agent is 5:3-5.
3. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The preparation method of the modified silver-cerium-zinc doped silicon dioxide comprises the following steps: S31, at room temperature, add 300 mL of tetra-n-butyl silicate to 400 mL of ethanol and stir for 40 min to form solution A; S32, adding 0.7 g of silver nitrate, 8 g of cerium nitrate and 15 g of zinc nitrate to a solution consisting of 300 mL of ethanol, 18 mL of acetic acid and 120 mL of water to form solution B; S33, adding solution B dropwise into solution A, stirring for 40 min, heating to 43° C., standing for 12 h, then centrifuging, washing, drying at 92° C. for 15 h, and finally calcining at 530° C. for 3 h, cooling, and grinding to obtain silver-cerium-zinc-doped silica; S34, mixing 0.8 g of vinyl triethoxysilane with 60 g of ethanol and 40 g of water, stirring evenly to obtain a mixture C; S35. Add the obtained silver-cerium-zinc doped silica to mixture C, then heat it to 40°C, stir it at 200 r / min for 150 min, and finally filter, wash, dry and grind it at 85°C to obtain modified silver-cerium-zinc doped silica, wherein the particle size of the modified silver-cerium-zinc doped silica is 30-50 nm.
4. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The preparation method of the cyclodextrin modified natural antibacterial agent is as follows: 5 parts of cyclodextrin and 30 parts of purslane powder with a particle size of 5-8 microns are put into a reactor according to their mass fractions, and then the temperature is raised to 40-50° C., and ultrasonic treatment is performed for 50-60 minutes at an ultrasonic power of 40 W, so that the cyclodextrin fully covers the purslane powder to obtain the cyclodextrin modified natural antibacterial agent.
5. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The preparation method of the degradable modified polyethylene resin comprises the following steps: S51. According to the mass fractions, 16.9 parts of 2-bromo-1,1-dimethoxyethane, 10.6 parts of 1,4-butanediol, 0.34 parts of p-toluenesulfonic acid and 45 parts of toluene were added into the reactor in sequence, the temperature was raised to 125°C, the mixture was stirred under reflux for 18-20 hours, and then washed with ethyl acetate for 3 times, and 2-bromo-1,3-dioxepane was obtained by vacuum distillation. Then 33 parts of tetrahydrofuran and 14.1 parts of potassium tert-butoxide were added, the mixture was stirred for 80-85 minutes, the temperature was lowered to room temperature, the reaction was continued with stirring for 14 hours, ether was added, the mixture was filtered, the mixture was washed with ether and filtered, and the filtrate was vacuum distilled to obtain an intermediate; S51. According to the mass proportions, 20.5 parts of the intermediate, 13.9 parts of N-vinylcaprolactam and 68.8 parts of toluene are added into the reactor, and then 8.34 parts of thiourea chitosan-Co (Ⅱ) complex and 0.28 parts of azobisisobutyronitrile are added. Ethylene is introduced under nitrogen protection at a pressure of 29 bar. The temperature is raised to 75°C, and the mixture is stirred and reacted for 24 hours. The solvent is removed by distillation under reduced pressure, and the filter cake is filtered. After washing three times with toluene, the filter cake is dried at 72°C for 24 hours to obtain a crude product. The crude product is pulverized and passed through a 100-mesh sieve to obtain a degradable modified polyethylene resin.
6. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The preparation method of the modified pigment comprises the following steps: S61. Add 10 parts of pigment and 3 parts of dimer acid polyester polyol to 20 parts of toluene according to the mass fractions, ultrasonically disperse for 30 minutes, add 6 parts of toluene-2,4 diisocyanate and 0.03 parts of dibutyltin dilaurate, stir mechanically to mix, transfer the system to a reactor at 63° C., react for 10 hours, filter, wash and dry after the reaction to obtain an isocyanate-activated pigment; S62. Add 10 parts of isocyanate-activated pigment to 25 parts of N,N-dimethylformamide in parts by mass, ultrasonicate for 30 minutes, add 15 parts of hydroxyl-terminated polysiloxane and 0.01 parts of dibutyltin dilaurate, stir and mix evenly, transfer to a reactor at 80°C, react for 3 hours, filter after the reaction is completed, wash the filter cake with ethanol, and vacuum dry to obtain a modified pigment.
7. The environmentally friendly antibacterial masterbatch according to claim 6, characterized in that: The pigment is one of titanium dioxide, red iron oxide and yellow iron oxide.
8. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010 , antioxidant 1076 and antioxidant 168 .
9. The environmentally friendly antibacterial masterbatch according to claim 1, characterized in that: The coupling agent is composed of vinyl triethoxysilane, γ-mercaptopropyl trimethoxysilane and γ-glycidyloxypropyl trimethoxysilane in a mass ratio of 3:4:
3.
10. A method for preparing an environmentally friendly antibacterial masterbatch as claimed in any one of claims 1 to 9, characterized in that: Linear low-density polyethylene, biodegradable modified polyethylene resin, modified pigment, antioxidant, polyethylene wax, composite antibacterial agent and coupling agent are sequentially added into an internal mixer for internal mixing at a temperature of 130° C. for a time of 10-20 min. After discharging, the material mass is added into a twin-screw extruder through a feeder for extrusion granulation at a temperature of 190-230° C. and a screw speed of 280-350 rpm to obtain an environmentally friendly antibacterial masterbatch.
Citation Information
Patent Citations
Polyethylene antibacterial mildew-resistant master batch and preparation method thereof
CN103881193A
Sterilization repairing cleaning agent, preparation method and application thereof
CN106109351A
Special antibacterial, water-repellent, stain-resistant and aging-resistant color master batch for fishing net line and preparation method thereof
CN109161089A
Color master batch with natural antibacterial function and preparation process thereof
CN113881206A
Polyethylene color master batch with low odor and high carbon black content and preparation method thereof
CN115160681A
Cited By
Permeable floor for upgrading renewable resources of wind power generation blades
CN119955197A