Matt master batch and preparation method thereof

By combining modified silica and oligopolymerized malting polyvinyl chloride resin, combined with maleic anhydride grafted polyethylene wax, an organic/inorganic three-dimensional network structure is formed, and the problem of poor compatibility between matte additives and plastic substrates is solved. It achieves efficient matte effect and material performance improvement.

CN118931040AInactive Publication Date: 2024-11-12FOSHAN XINRONG NEW MATERIAL CO LTD
View PDF 0 Cites 4 Cited by

Patent Information

Application Number
CN202411193980.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing matte additives have poor compatibility with plastic substrates, which are prone to agglomeration and uneven distribution, affecting the toughness, mechanical strength and thermal stability of the plastic.

Method used

Modified silica and oligopolymerized malting polyvinyl chloride resin are used to modify silica by silane coupling agent and maleic anhydride/hydroxyethyl methacrylate to increase the surfactant carbon carbon double bond and organic functional groups. Combined with maleic anhydride grafted polyethylene wax, an organic/inorganic three-dimensional network structure is formed to improve compatibility and dispersion.

Benefits of technology

The matte effect is improved, the toughness, mechanical strength and thermal stability of the product are guaranteed, the agglomeration is avoided, and the scattering and diffuse reflection effect of light is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005015833070000111
    Figure BDA0005015833070000111
Patent Text Reader

Abstract

The invention relates to the technical field of high polymer material preparation, in particular to a matte master batch and a preparation method thereof. The matt master batch comprises the following raw material components in parts by mass: 40-60 parts of a resin carrier, 1-5 parts of a dispersing agent A, 1-3 parts of an antioxidant and 13-41 parts of a matting composition, wherein the matting composition comprises the following raw material components in percentage by mass: 40%-60% of modified silicon dioxide, 30%-50% of matting polyvinyl chloride resin and 5%-10% of a compatilizer; the modified silicon dioxide is prepared by modifying silicon dioxide with a silane coupling agent and maleic anhydride / hydroxyethyl methylacrylate; the polymerization degree of the extinction polyvinyl chloride resin is less than or equal to 700, and the gel content is 25-30%; the compatilizer is maleic anhydride grafted polyethylene wax. The matt master batch is good in matt effect, the dispersity and compatibility of all the components are good, agglomeration is not prone to occurring, and the toughness, mechanical strength, heat stability and other use performance of a product are effectively guaranteed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer material preparation, and in particular to a matte masterbatch and a preparation method thereof. Background Art

[0002] Plastic products are widely used in packaging, automobiles, electronics, construction, textiles and many other fields due to their excellent mechanical and optical properties. Gloss, as an important indicator of optical properties, directly affects the appearance and texture of the product. Too high gloss may damage the visual effect of the product, thereby reducing the commercial value of the product. Therefore, in the research and development stage of plastic products, the control of gloss becomes an important task.

[0003] At present, the main method to reduce gloss is to add matte additives. The main function of matte agents is to increase the roughness of the material surface, enhance light scattering and reduce reflection, thereby achieving the effect of reducing gloss. However, this method has some problems in practical applications, such as the poor compatibility of traditional matte additives with plastic substrates, easy accumulation and agglomeration, and uneven distribution, which in turn affects the homogeneity and stability of the matte effect. In addition, the interaction between matte additives and plastic substrates may also cause the breakage or rearrangement of plastic molecular chains, thereby affecting the toughness, mechanical strength, thermal stability and other performance of the plastic. Therefore, in order to obtain high-quality, high-matte plastic products, it is necessary to comprehensively consider various factors, including the selection of matte additives, compatibility with plastic substrates, dispersibility, and its impact on plastic properties. Summary of the invention

[0004] In view of this, the present invention provides a matte masterbatch and a preparation method thereof. The matte masterbatch has good matte effect, and the components have good dispersibility and compatibility and are not easy to agglomerate, thereby effectively ensuring the toughness, mechanical strength, thermal stability and other performance of the product.

[0005] In a first aspect, the present invention provides a matte masterbatch, comprising the following raw material components in parts by weight: 40-60 parts of a resin carrier, 1-5 parts of a dispersant A, 1-3 parts of an antioxidant, and 13-41 parts of a matte composition; wherein the matte composition comprises the following raw material components in parts by weight: 40%-60% of modified silica, 30%-50% of a matte polyvinyl chloride resin, and 5%-10% of a compatibilizer; the modified silica is prepared by modifying silica with a silane coupling agent and maleic anhydride / hydroxyethyl methacrylate; the matte polyvinyl chloride resin has a degree of polymerization of ≤700 and a gel content of 25%-30%; and the compatibilizer is maleic anhydride grafted polyethylene wax.

[0006] Silicon dioxide has a porous structure, adjustable particle size, easy modification, low energy consumption, and strong chemical inertness and refractive index similar to ordinary resins, and is a commonly used matting additive. However, there are unsaturated residual bonds and hydroxyl groups in different bonding states on the surface of silicon dioxide, which are easy to reunite, and have poor compatibility with plastic substrates, thereby affecting the toughness, mechanical strength and thermal stability of the product. The present invention uses silane coupling agent and maleic anhydride / hydroxyethyl methacrylate to surface-modify silicon dioxide, which can not only reduce the hydroxyl content on the surface of silicon dioxide, but also make its surface change from polarity to non-polarity, effectively avoid reunion, and can also introduce active carbon-carbon double bonds and organic functional groups into the surface of silicon dioxide, thereby improving the interface compatibility with plastic substrates. At the same time, organic segments coat silicon dioxide particles therein, so that the modified silicon dioxide particle size is large, and a rough structure is better formed, which is conducive to the random reflection of light and improves the matting effect.

[0007] The present invention adds a matte polyvinyl chloride resin with a low degree of polymerization, has a small molecular weight, a low melting and gelling temperature of the material, and a specific gel content so that it has good resin particle size regularity and plasticizing performance, and is particularly suitable for injection molding. In addition, the carbon-carbon double bonds on the surface of the modified silicon dioxide can undergo a condensation reaction with the double bonds in the matte polyvinyl chloride resin to form a three-dimensional network structure, thereby enhancing the interface bonding between the two, hindering the thermal decomposition rate of the polymer molecular chain, and thus improving the mechanical strength and thermal stability of the material.

[0008] The invention adds a specific amount of a compatibilizer maleic anhydride grafted polyethylene wax, which has a maleic anhydride polar group and can not only improve the compatibility among silicon dioxide, matte polyvinyl chloride resin and plastic substrate to form an organic / inorganic three-dimensional network hybrid structure, but also improve the dispersibility of silicon dioxide, help to form a rough surface at a microscopic scale, so as to enhance the refraction and diffuse reflection after the scattering of light, thereby greatly reducing the surface gloss of the product.

[0009] Optionally, the preparation method of the modified silicon dioxide comprises the following steps:

[0010] Step S1, weighing 3-6 parts of silicon dioxide in parts by weight and dispersing them in ethyl acetate, then adding 30-40 parts of a silane coupling agent and deionized water, stirring and reacting at a temperature of 60-100° C. for 8-16 hours, filtering, washing, and drying to obtain silane coupling agent-modified silicon dioxide;

[0011] Step S2, weighing 30-40 parts of maleic anhydride, 50-60 parts of hydroxyethyl methacrylate, 0.4-0.8 parts of tetrabutylammonium bromide and 0.2-0.4 parts of p-hydroxyanisole, mixing them evenly, stirring and reacting them at 80-100° C. for 4-6 hours, adding 3-6 parts of silane coupling agent modified silica, continuing to react at 80-100° C. for 8-12 hours, filtering, washing and drying the product to obtain modified silica.

[0012] Optionally, the method for preparing the matte polyvinyl chloride resin comprises the following steps:

[0013] According to weight parts, 100-200 parts of deionized water, 80-100 parts of vinyl chloride, 0.5-1 parts of dispersant B, 3-4 parts of matting agent and 0.01-0.05 parts of pH regulator are added to the reaction kettle in sequence and mixed evenly, and then 0.1-0.3 parts of initiator are added to carry out constant temperature polymerization reaction at 60-61°C, and when the reaction pressure drops to 0.08-0.1Mpa, 0.1-0.2 parts of terminator are added to discharge the material, residual vinyl chloride is removed by steam stripping, and water is removed by centrifugal drying to obtain matt polyvinyl chloride resin.

[0014] Optionally, the matting agent is a composite of diallyl phthalate and ethylene glycol dimethacrylate, wherein the mass ratio of diallyl phthalate to ethylene glycol dimethacrylate is 2.8-3.2:5.

[0015] Optionally, the initiator is selected from at least one of dicyclohexyl peroxydicarbonate, isopropyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, dibenzoyl peroxide, dodecyl peroxide, benzoyl peroxide, lauroyl peroxide, acetylcyclohexanesulfonyl peroxide, azobisisoheptanenitrile, azobisisobutyronitrile, sodium persulfate, potassium persulfate, ammonium persulfate, di-tert-butyl peroxide, diisopropyl peroxide, tert-butyl perbenzoate or tert-butyl pervalerate.

[0016] Optionally, the dispersant B is selected from polyvinyl alcohol having a degree of alcoholysis of 50-90.

[0017] Optionally, the terminator is selected from at least one of N,N-diethylhydroxylamine, α-methylstyrene, asymmetric hindered phenol antioxidant 245, p-tert-butylcatechol, sodium dimethyldithiocarbamate, sodium polysulfide, hydroquinone or nonylphenol.

[0018] Optionally, the pH regulator is selected from at least one of sodium hydride, ammonium bicarbonate, sodium bicarbonate, and ammonia water.

[0019] Optionally, the silane coupling agent is selected from at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane.

[0020] Optionally, the antioxidant is selected from at least one of antioxidant 1010, antioxidant 168 or bis(3,5-tert-butyl-4-hydroxyphenyl)sulfide.

[0021] Optionally, the dispersant A is selected from at least one of polyethylene wax, calcium stearate or hexenyl bisstearamide.

[0022] Optionally, the resin carrier is selected from at least one of polypropylene, polyethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polystyrene, ABS, polymethyl methacrylate, polyimide or polycarbonate.

[0023] In a second aspect, the present invention also provides a method for preparing the matte masterbatch, the preparation method comprising the following steps:

[0024] Step a, weighing each component according to the ratio, drying the matte polyvinyl chloride resin and the compatibilizer at 40-60° C. for 2-3 hours, mixing them evenly, then heating them to 110-130° C., adding modified silicon dioxide, mixing them evenly, crushing, and sieving to obtain the matte composition;

[0025] Step b: uniformly mixing the resin matrix, dispersant, antioxidant and matte composition, melt blending, extruding and granulating, to obtain the matte masterbatch.

[0026] In a third aspect, the present invention also provides the application of the matte masterbatch in the field of plastic sheets and films.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The matte masterbatch provided by the present invention is added with modified silicon dioxide, matte polyvinyl chloride resin and compatibilizer maleic anhydride grafted polyethylene wax, which has a synergistic effect and good matte effect, and each component has good dispersibility and compatibility and is not easy to agglomerate, thereby effectively ensuring the toughness, mechanical strength, thermal stability and other use properties of the product. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail in conjunction with the following embodiments. Unless otherwise defined, all professional terms used hereinafter have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention. Unless otherwise specified, the various reagents and raw materials used in the present invention are all commodities that can be purchased from the market or products that can be prepared by known methods. In the present invention, the average particle size (D50) of the silicon dioxide used is 2.5μm, and the mass fraction is 98.00%; polyethylene wax and maleic anhydride grafted polyethylene wax, with a mass fraction of 99.00%, are purchased from Qingdao Sino New Materials Co., Ltd.; the polyvinyl alcohol is purchased from Japan Synthetic Chemical.

[0030] In order to better illustrate the present invention, further examples are given below.

[0031] Example 1

[0032] This embodiment provides a matte masterbatch, comprising the following raw material components in parts by weight: 50 parts of a resin carrier (polypropylene), 3 parts of a dispersant A (polyethylene wax), 2 parts of an antioxidant (antioxidant 1010), and 24 parts of a matte composition.

[0033] The matte composition comprises the following raw material components in the following mass percentages: 50% modified silicon dioxide, 42% matte polyvinyl chloride resin, and 8% compatibilizer; the modified silicon dioxide is prepared by modifying silicon dioxide with a silane coupling agent and maleic anhydride / hydroxyethyl methacrylate; the degree of polymerization of the matte polyvinyl chloride resin is ≤700, and the gel content is 25%-30%; the compatibilizer is maleic anhydride grafted polyethylene wax.

[0034] Among them, the matte masterbatch is prepared by the following scheme:

[0035] Step S1, weighing 3-6 parts of silicon dioxide in parts by weight and dispersing them in ethyl acetate, then adding 30-40 parts of a silane coupling agent (γ-aminopropyltriethoxysilane) and deionized water, stirring and reacting at 80° C. for 12 hours, filtering, washing, and drying to obtain silane coupling agent-modified silicon dioxide;

[0036] Step S2, weighing 35 parts of maleic anhydride, 55 parts of hydroxyethyl methacrylate, 0.6 parts of tetrabutylammonium bromide and 0.3 parts of p-hydroxyanisole, mixing them evenly, stirring and reacting them at 90° C. for 5 hours, adding 4 parts of silane coupling agent-modified silica, and continuing to react at 90° C. for 10 hours, filtering, washing and drying the product to obtain modified silica;

[0037] Step S3, according to weight parts, add 150 parts of deionized water, 90 parts of vinyl chloride, 0.8 parts of dispersant B (polyvinyl alcohol), 3.5 parts of matting agent (complex of diallyl phthalate and ethylene glycol dimethacrylate in a mass ratio of 3:5) and 0.03 parts of pH regulator (sodium bicarbonate) to the reactor in sequence, mix them evenly, then add 0.2 parts of initiator (dicyclohexyl peroxydicarbonate), carry out constant temperature polymerization reaction at 60.5°C, when the reaction pressure drops to 0.1Mpa, add 0.15 parts of terminator (N,N-diethylhydroxylamine) to discharge, remove residual vinyl chloride by steam stripping, and remove water by centrifugal drying to obtain matte polyvinyl chloride resin;

[0038] Step S4, weighing each component according to the ratio, drying the matte polyvinyl chloride resin and the compatibilizer at 50° C. for 2.5 hours, mixing them evenly, then heating to 120° C., adding modified silicon dioxide, mixing them evenly, crushing, and passing through a 50-mesh sieve to obtain the matte composition;

[0039] Step S5, mix the resin matrix, dispersant A, antioxidant and matting composition evenly, heat to 110°C and stir for 25 minutes, and then enter the extruder for extrusion. The temperature of the extruder is set as follows: 170°C in zone 1, 190°C in zone 2, 200°C in zones 3 to 6, 210°C in zone 7, 220°C in zone 8, and 210°C in die head to obtain the matte masterbatch.

[0040] Example 2

[0041] The present embodiment provides a matte masterbatch, comprising the following raw material components in parts by weight: 40 parts of a resin carrier (polymethyl methacrylate), 1 part of a dispersant A (calcium stearate), 1-3 parts of an antioxidant (antioxidant 168), and 13-41 parts of a matte composition.

[0042] The matte composition comprises the following raw material components in the following mass percentages: 40% modified silica, 50% matte polyvinyl chloride resin, and 10% compatibilizer; the modified silica is prepared by modifying silica with a silane coupling agent and maleic anhydride / hydroxyethyl methacrylate; the degree of polymerization of the matte polyvinyl chloride resin is ≤700, and the gel content is 25%-30%; the compatibilizer is maleic anhydride grafted polyethylene wax.

[0043] Among them, the matte masterbatch is prepared by the following scheme:

[0044] Step S1, weighing 3 parts of silicon dioxide in parts by weight and dispersing them in ethyl acetate, then adding 30 parts of a silane coupling agent (γ-glycidyloxypropyltrimethoxysilane) and deionized water, stirring and reacting at 60° C. for 8 hours, filtering, washing, and drying to obtain silane coupling agent-modified silicon dioxide;

[0045] Step S2, weighing 30 parts of maleic anhydride, 50 parts of hydroxyethyl methacrylate, 0.4 parts of tetrabutylammonium bromide and 0.2 parts of p-hydroxyanisole, mixing them evenly, stirring and reacting them at 80° C. for 4 hours, adding 3 parts of silane coupling agent-modified silica, and continuing to react at 80° C. for 8 hours, filtering, washing and drying the product to obtain modified silica;

[0046] Step S3, according to weight parts, add 100 parts of deionized water, 80 parts of vinyl chloride, 0.5 parts of dispersant B (polyvinyl alcohol), 3 parts of matting agent (a composite of diallyl phthalate and ethylene glycol dimethacrylate in a mass ratio of 2.8:5) and 0.01 parts of pH regulator (sodium bicarbonate) to the reactor in sequence, mix them evenly, then add 0.1 parts of initiator (dicyclohexyl peroxydicarbonate), carry out constant temperature polymerization at 60°C, when the reaction pressure drops to 0.08Mpa, add 0.1 parts of terminator (N,N-diethylhydroxylamine) to discharge, remove residual vinyl chloride by steam stripping, and remove moisture by centrifugal drying to obtain matte polyvinyl chloride resin;

[0047] Step S4, weighing each component according to the ratio, drying the matte polyvinyl chloride resin and the compatibilizer at 40° C. for 2 h, mixing them evenly, then heating to 110° C., adding modified silicon dioxide, mixing them evenly, crushing, and passing through a 50-mesh sieve to obtain the matte composition;

[0048] Step S5, mix the resin matrix, dispersant A, antioxidant and matting composition evenly, heat to 110°C and stir for 25 minutes, and then enter the extruder for extrusion. The temperature of the extruder is set as follows: 170°C in zone 1, 230°C in zone 2, 200°C in zones 3 to 6, 210°C in zone 7, 220°C in zone 8, and 230°C in die head to obtain the matte masterbatch.

[0049] Example 3

[0050] The present embodiment provides a matte masterbatch, comprising the following raw material components in parts by weight: 60 parts of a resin carrier (polyethylene terephthalate), 5 parts of a dispersant A (hexenyl bisstearamide), 3 parts of an antioxidant (antioxidant 168), and 41 parts of a matte composition.

[0051] The matte composition comprises the following raw material components in the following mass percentages: 60% modified silica, 30% matte polyvinyl chloride resin, and 10% compatibilizer; the modified silica is prepared by modifying silica with a silane coupling agent and maleic anhydride / hydroxyethyl methacrylate; the degree of polymerization of the matte polyvinyl chloride resin is ≤700, and the gel content is 30%; the compatibilizer is maleic anhydride grafted polyethylene wax.

[0052] Among them, the matte masterbatch is prepared by the following scheme:

[0053] Step S1, according to weight parts, weigh 6 parts of silicon dioxide and disperse them in ethyl acetate, then add 40 parts of silane coupling agent (γ-aminopropyltrimethoxysilane) and deionized water, stir and react at 100° C. for 16 hours, filter, wash and dry to obtain silane coupling agent modified silicon dioxide;

[0054] Step S2, weighing 40 parts of maleic anhydride, 60 parts of hydroxyethyl methacrylate, 0.8 parts of tetrabutylammonium bromide and 0.4 parts of p-hydroxyanisole, mixing them evenly, stirring and reacting them at 100° C. for 6 hours, adding 6 parts of silane coupling agent-modified silica, and continuing to react at 100° C. for 12 hours, filtering, washing and drying the product to obtain modified silica;

[0055] Step S3, according to weight parts, add 200 parts of deionized water, 100 parts of vinyl chloride, 1 part of dispersant B (polyvinyl alcohol), 4 parts of matting agent (a composite of diallyl phthalate and ethylene glycol dimethacrylate in a mass ratio of 3.2:5) and 0.05 parts of pH regulator (sodium bicarbonate) to the reactor in sequence, mix them evenly, then add 0.3 parts of initiator (dibenzoyl peroxide), and carry out constant temperature polymerization at 61° C. When the reaction pressure drops to 0.1 MPa, add 0.2 parts of terminator (sodium dimethyldithiocarbamate) to discharge the material, remove residual vinyl chloride by steam stripping, and remove moisture by centrifugal drying to obtain matte polyvinyl chloride resin;

[0056] Step S4, weighing each component according to the ratio, drying the matte polyvinyl chloride resin and the compatibilizer at 60° C. for 3 h, mixing them evenly, then heating to 130° C., adding modified silicon dioxide, mixing evenly, crushing, and passing through a 100-mesh sieve to obtain the matte composition;

[0057] Step S5, mix the resin matrix, dispersant A, antioxidant and matte composition evenly, heat to 110°C and stir for 25 minutes, and then enter the twin-screw extruder for extrusion. The temperature of the extruder is set as follows: 200°C in zone 1, 260°C in zone 2, the temperatures of zones 3 to 6 are all 250°C, the temperature of zone 7 is 240°C, the temperature of zone 8 is 250°C, and the head temperature is 250°C to obtain the matte masterbatch.

[0058] Comparative Example 1

[0059] This comparative example provides a matte masterbatch, and its preparation process is the same as that of Example 1, except that an equal amount of silicon dioxide is used to replace modified silicon dioxide.

[0060] Comparative Example 2

[0061] This comparative example provides a matte masterbatch, and its preparation process is the same as that of Example 1, except that an equal amount of polyethylene wax is used to replace the maleic anhydride grafted polyethylene wax.

[0062] The matte masterbatch prepared in Examples 1-3 and Comparative Examples 1-2 was injection molded by an injection molding machine to obtain test specimens (including dumbbell-shaped test specimens and strip-shaped test specimens), the thickness of the test specimens was 0.5 mm, and was used for the following experimental tests.

[0063] (1) Mechanical properties test: With reference to the national standard GB / T 1040.1-2018 "Test of tensile properties of plastics", a microcomputer-controlled electronic universal testing machine, model: TMS-D10H, was used to test the tensile strength; with reference to the national standard GB / T1043.1-2008 "Determination of impact properties of simply supported beams of plastics - Part 1" was used to test the impact strength (unnotched specimen).

[0064] (2) Haze and transmittance: Refer to GB / T 2410-2008 "Determination of light transmittance and haze of transparent plastics" to test the light transmittance and haze.

[0065] (3) Glossiness: Glossiness was tested according to the national standard GB / T 8807-1988, with a measuring angle of 45°. The test results are shown in Table 1.

[0066] Table 1

[0067]

[0068] In summary, the matte masterbatch prepared by the present invention has a synergistic effect among the components, has a good matte effect, and has good dispersibility and compatibility of the components, is not easy to agglomerate, effectively guarantees the mechanical properties of the product, and has broad application prospects.

[0069] The embodiments described above only express several preferred embodiments of the present invention, and the descriptions thereof are relatively specific and detailed, but are not intended to limit the present invention. It should be noted that for those skilled in the art, the present invention may also have various changes and modifications, and any modifications, equivalent substitutions, improvements, etc. made within the concept and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A matte masterbatch, characterized in that: The method comprises the following raw material components in parts by weight: 40-60 parts of a resin carrier, 1-5 parts of a dispersant A, 1-3 parts of an antioxidant, and 13-41 parts of a matting composition; The matte composition comprises the following raw material components in the following mass percentages: 40%-60% of modified silicon dioxide, 30%-50% of matte polyvinyl chloride resin, and 5%-10% of a compatibilizer; the modified silicon dioxide is prepared by modifying silicon dioxide with a silane coupling agent and maleic anhydride / hydroxyethyl methacrylate; the degree of polymerization of the matte polyvinyl chloride resin is ≤700, and the gel content is 25%-30%; and the compatibilizer is maleic anhydride grafted polyethylene wax.

2. The matte masterbatch according to claim 1, characterized in that: The preparation method of the modified silicon dioxide comprises the following steps: Step S1, weighing 3-6 parts of silicon dioxide in parts by weight and dispersing them in ethyl acetate, then adding 30-40 parts of a silane coupling agent and deionized water, stirring and reacting at a temperature of 60-100° C. for 8-16 hours, filtering, washing, and drying to obtain silane coupling agent-modified silicon dioxide; Step S2, weighing 30-40 parts of maleic anhydride, 50-60 parts of hydroxyethyl methacrylate, 0.4-0.8 parts of tetrabutylammonium bromide and 0.2-0.4 parts of p-hydroxyanisole, mixing them evenly, stirring and reacting them at 80-100° C. for 4-6 hours, adding 3-6 parts of silane coupling agent modified silica, continuing to react at 80-100° C. for 8-12 hours, filtering, washing and drying the product to obtain modified silica.

3. The matte masterbatch according to claim 1, characterized in that: The preparation method of the matte polyvinyl chloride resin comprises the following steps: According to weight parts, 100-200 parts of deionized water, 80-100 parts of vinyl chloride, 0.5-1 parts of dispersant B, 3-4 parts of matting agent and 0.01-0.05 parts of pH regulator are added to the reaction kettle in sequence and mixed evenly, and then 0.1-0.3 parts of initiator are added to carry out constant temperature polymerization reaction at 60-61°C, and when the reaction pressure drops to 0.08-0.1Mpa, 0.1-0.2 parts of terminator are added to discharge the material, residual vinyl chloride is removed by steam stripping, and water is removed by centrifugal drying to obtain matt polyvinyl chloride resin.

4. The matte masterbatch according to claim 3, characterized in that: The matting agent is a composite of diallyl phthalate and ethylene glycol dimethacrylate, wherein the mass ratio of diallyl phthalate to ethylene glycol dimethacrylate is 2.8-3.2:

5.

5. The matte masterbatch according to claim 3, characterized in that: The initiator is selected from at least one of dicyclohexyl peroxydicarbonate, isopropyl peroxyneodecanoate, tert-butyl peroxyneodecanoate, dibenzoyl peroxide, dodecyl peroxide, benzoyl peroxide, lauroyl peroxide, acetylcyclohexanesulfonyl peroxide, azobisisoheptanenitrile, azobisisobutyronitrile, sodium persulfate, potassium persulfate, ammonium persulfate, di-tert-butyl peroxide, diisopropyl peroxide, tert-butyl perbenzoate or tert-butyl peroxyvalerate; and / or The dispersant B is selected from polyvinyl alcohol having an alcoholysis degree of 50-90; and / or The terminator is selected from at least one of N,N-diethylhydroxylamine, α-methylstyrene, asymmetric hindered phenol antioxidant 245, p-tert-butylcatechol, sodium dimethyldithiocarbamate, sodium polysulfide, hydroquinone or nonylphenol; and / or The pH regulator is selected from at least one of sodium hydride, ammonium bicarbonate, sodium bicarbonate, and ammonia water.

6. The matte masterbatch according to claim 1, characterized in that: The silane coupling agent is selected from at least one of γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane or N-β-(aminoethyl)-γ-aminopropylmethyldimethoxysilane.

7. The matte masterbatch according to claim 1, characterized in that: The antioxidant is selected from at least one of antioxidant 1010, antioxidant 168 or bis(3,5-tert-butyl-4-hydroxyphenyl)sulfide; and / or The dispersant A is selected from at least one of polyethylene wax, calcium stearate or hexenyl bisstearamide.

8. The matte masterbatch according to claim 1, characterized in that: The resin carrier is selected from at least one of polypropylene, polyethylene, polyamide, polyethylene terephthalate, polybutylene terephthalate, polyvinyl chloride, polystyrene, ABS, polymethyl methacrylate, polyimide or polycarbonate.

9. A method for preparing the matte masterbatch according to any one of claims 1 to 8, characterized in that: The steps include: Step a, weighing each component according to the ratio, drying the matte polyvinyl chloride resin and the compatibilizer at 40-60° C. for 2-3 hours, mixing them evenly, then heating them to 110-130° C., adding modified silicon dioxide, mixing them evenly, crushing, and sieving to obtain the matte composition; Step b: uniformly mixing the resin matrix, dispersant, antioxidant and matte composition, melt blending, extruding and granulating, to obtain the matte masterbatch.

10. Use of the matte masterbatch according to any one of claims 1 to 8 in the field of plastic plates and films.

Citation Information

Cited By

  • Plastic film with extinction effect and preparation method thereof

    CN119371743A

  • Matt film and preparation method thereof

    CN120775355A

  • Master batch slice for polyester matte film as well as preparation method and application of master batch slice

    CN121108694A

  • PVC matt film and preparation method thereof

    CN122278083A