PP / HDPE (polypropylene / high-density polyethylene) plastic for automotive trim and preparation method of PP / HDPE plastic

By introducing polypropylene, ethylene propylene ternary rubber, high-density polyethylene and other components into PP/HDPE plastics, and through modification treatment, the problem of poor compatibility between PP and HDPE plastics is solved, and the mechanical properties of composite materials are improved and durability, especially in high temperature and shock conditions.

CN118931044AInactive Publication Date: 2024-11-12QINGDAO MINGRUIXIANG PLASTICS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411241269.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The poor compatibility of PP and HDPE plastics leads to insufficient mechanical properties and durability of composite materials, especially poor performance in high temperatures and external impacts.

Method used

Composite materials using polypropylene, ethylene propylene ternary rubber, high-density polyethylene, modified walnut shell powder, nanoceramic particles, modified glass fiber, anti-aging agent and coupling agent, and grafting through maleic anhydride Modification treatments such as polypropylene and chitosan solutions enhance interface adhesion and dispersion, and improve the impact, wear and thermal stability of the material.

Benefits of technology

It significantly improves the impact resistance, heat resistance and mechanical properties of PP/HDPE plastics, so that they maintain good performance in high temperature environments, extend their service life, and reduce the risk of electrostatic discharge.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005029351740000101
    Figure BDA0005029351740000101
  • Figure BDA0005029351740000111
    Figure BDA0005029351740000111
Patent Text Reader

Abstract

The invention relates to the technical field of plastics, and particularly discloses a PP / HDPE (Polypropylene / High-Density Polyethylene) plastic for automotive interiors and a preparation method of the PP / HDPE plastic. The PP / HDPE plastic for the automotive trim comprises the following raw materials in parts by weight: 80-90 parts of polypropylene, 15-18 parts of ethylene propylene diene monomer, 30-35 parts of high density polyethylene, 25-28 parts of modified walnut shell powder, 2-3 parts of an anti-aging agent, 2-5 parts of maleic anhydride grafted polypropylene, 6-9 parts of nano ceramic particles, 1-3 parts of a coupling agent, 16-18 parts of modified glass fibers, 0.3-0.5 part of an antistatic agent and 10-15 parts of talcum powder. According to the PP / HDPE plastic for the automotive trim, the compatibility of PP and HDPE is relatively good, and the plastic has relatively good mechanical properties such as mechanical property, flexibility, wear resistance and the like, so that the plastic has relatively good durability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of plastics, and more specifically, to a PP / HDPE plastic for automobile interior decoration and a preparation method thereof. Background Art

[0002] Polypropylene, abbreviated as PP, is a common thermoplastic plastic made from propylene monomer through polymerization reaction. It has low density, chemical resistance, heat resistance and good mechanical properties. It is widely used in packaging, textiles, automobiles, home appliances, medical care, construction and other fields.

[0003] High-density polyethylene, referred to as HDPE, is a linear thermoplastic made from ethylene monomers through high-pressure or low-pressure polymerization. It has high tensile strength, rigidity, chemical resistance and heat resistance. It is widely used in packaging, pipes, containers, films, fibers, medical treatment, construction and other fields.

[0004] At present, PP / HDPE plastics obtained by compounding the two have been widely used. They have good heat resistance, cold resistance and chemical stability. However, the compatibility of PP and HDPE is poor. Due to their different chemical structures and crystallinity, direct mixing may lead to weak interfacial adhesion, which in turn affects the mechanical properties and durability of the composite material. Summary of the invention

[0005] In order to improve the poor compatibility between PP and HDPE, which in turn affects the mechanical properties and durability of the composite material, the present application provides a PP / HDPE plastic for automotive interior and a preparation method thereof.

[0006] In the first aspect, the present application provides a PP / HDPE plastic for automobile interior, adopting the following technical scheme: a PP / HDPE plastic for automobile interior, comprising the following raw materials, measured by weight: 80-90 parts of polypropylene, 15-18 parts of EPDM rubber, 30-35 parts of high-density polyethylene, 25-28 parts of modified walnut shell powder, 2-3 parts of anti-aging agent, 2-5 parts of maleic anhydride grafted polypropylene, 6-9 parts of nano-ceramic particles, 1-3 parts of coupling agent, 16-18 parts of modified glass fiber, 0.3-0.5 parts of antistatic agent, and 10-15 parts of talc.

[0007] By adopting the above technical scheme, polypropylene has good chemical stability and mechanical properties, enhances the rigidity of PP / HDPE blends, makes it difficult to deform when under pressure, improves the heat resistance of PP / HDPE blends, makes it still maintain good performance in high temperature environments, improves the impact resistance of PP / HDPE, and makes it difficult to break when subjected to external force impact. EPDM rubber has excellent weather resistance, chemical resistance and heat resistance, significantly improves the impact resistance of PP / HDPE blends, and makes it difficult to break when subjected to external force impact. Polypropylene and EPDM rubber are mixed to improve the impact resistance, elasticity and low-temperature toughness of the material, while maintaining the rigidity and thermal stability of polypropylene.

[0008] High-density polyethylene has high strength, tolerance and tear resistance, which can enhance the mechanical properties and chemical stability of PP / HDPE blends and reduce cracks caused by environmental stress. The mixture of high-density polyethylene, EPDM rubber and polypropylene enhances the mechanical strength and chemical stability of the material, has good resistance to environmental stress cracking, can increase the service life of the blend in complex environments, and reduce cracks caused by stress. Maleic anhydride grafted polypropylene is used as a compatibilizer to make polypropylene and high-density polyethylene mix evenly, enhance interfacial adhesion, improve the compatibility between polypropylene and high-density polyethylene, and improve the mechanical properties and durability of the composite material.

[0009] Modified walnut shell powder has high hardness, good thermal stability and rigidity. It is added to PP / HDPE plastic to improve the hardness and wear resistance of the material, making it more durable during use, improve the heat resistance of PP / HDPE plastic, so that it can still maintain good performance in high temperature environment, enhance the rigidity of PP / HDPE plastic, improve its bending strength, and make it less likely to deform when under pressure. Anti-aging agents can delay the performance degradation of PP / HDPE plastic caused by oxidation during processing and use, and extend the service life of plastic products.

[0010] Nano-ceramic particles have good thermal stability, high hardness and strength, which can improve the hardness, rigidity, wear resistance and impact resistance of composite materials and extend the service life of materials; nano-ceramic particles can be loaded on the surface and pores of modified walnut shell powder, improve the hardness, strength, good thermal stability and wear resistance of polypropylene, and can enhance the tensile strength, compressive strength and impact resistance of polypropylene, making it more durable. Talc has good lubricity, which can improve the fluidity of plastic melt, make the various components mix evenly, improve the hardness, rigidity and impact resistance of plastic, and enhance the mechanical properties of materials.

[0011] Coupling agents can enhance the interface bonding between modified glass fiber, talcum powder and PP / HDPE matrix, improve the dispersion and compatibility of fillers in the plastic matrix, and improve the thermal stability of composite materials. Modified glass fiber has good strength, wear resistance and toughness. It cooperates with modified walnut shell powder and nano-ceramic particles to enhance the tensile strength, compressive strength, tear resistance and impact resistance of PP / HDPE plastics, making them more durable. Antistatic agents can reduce the resistance of plastic surfaces, reduce the accumulation of static charges, and prevent static discharge, thereby avoiding safety hazards such as fire and explosion caused by static electricity.

[0012] Optionally, the preparation method of the modified walnut shell powder comprises the following steps: (1) grinding walnut shells, dispersing them in deionized water, stirring them at 80-85° C. for 10-15 minutes, adding sodium hydroxide, continuing to stir for 30-35 minutes, filtering, and drying to obtain pretreated walnut shell powder; (2) dispersing nano-silica in a sulfuric acid solution, soaking for 25-30 minutes, washing with water, and filtering to obtain pretreated nano-silica; (3) dispersing the pretreated walnut shell powder of step (1) in deionized water, adding the pretreated nano-silica of step (2), stirring evenly, adding straw fiber filaments, stirring evenly, filtering, drying to obtain a mixture, spraying chitosan solution on the surface of the mixture, and drying to obtain modified walnut shell powder.

[0013] By adopting the above technical solution, the walnut shells are ground and sodium hydroxide is added. The sodium hydroxide corrodes the surface of the walnut shells, removes impurities in the walnut shells, increases the porosity of the walnut shells, increases the adsorption of the walnut shells, and helps to mix walnut powder with other components.

[0014] Nano-silica has high hardness, good dispersibility, and excellent thermal stability. It can improve the tensile strength, impact resistance, wear resistance, and scratch resistance of plastics. Nano-silica is treated with sulfuric acid to remove impurities on the surface of nano-silica and improve its dispersibility, which helps to evenly disperse nano-silica in walnut powder, thereby helping to improve the corresponding properties of walnut powder.

[0015] Pretreated walnut shell powder and pretreated nano-silicon dioxide are mixed. Nano-silicon dioxide can be loaded on the surface and pores of walnut powder. Pretreated walnut shell powder has good mechanical properties and high porosity. Nano-silicon dioxide has high specific surface area, good dispersibility and chemical stability. The two are mixed to improve the tensile strength, toughness, impact resistance, wear resistance and scratch resistance of walnut powder. Straw fiber has high porosity, flexibility and tensile strength. Walnut shell powder loaded with nano-silicon dioxide can be loaded on the surface and pores of straw fiber to improve the strength of straw fiber. It can be subsequently applied to plastics to improve the corresponding properties of plastics.

[0016] Chitosan solution is sprayed on the surface of the mixture. The chitosan solution has certain viscosity, film-forming properties, heat resistance and mechanical properties. It can cover the straw fiber filaments, so that the straw fiber filaments, nano-silicon dioxide and walnut shell powder are tightly bonded, thereby improving the mechanical properties of the modified walnut shell powder. It can be subsequently applied to plastics to improve the mechanical properties and wear resistance of the plastics.

[0017] Optionally, the mass ratio of the walnut shell, nano-silicon dioxide and straw fiber is 1:0.3-0.5:0.1-0.2.

[0018] By adopting the above technical solution, the mass ratio of walnut shell, nano-silicon dioxide and straw fiber is further limited within a certain range, and the tensile strength, toughness, impact resistance, wear resistance and scratch resistance of the modified walnut shell are improved. Nano-silicon dioxide can be loaded on the surface and pores of walnut powder, and walnut shell powder loaded with nano-silicon dioxide can be loaded on the surface and pores of straw fiber. Walnut shell, nano-silicon dioxide and straw fiber have a synergistic effect, which can be subsequently applied to plastics to improve the corresponding properties of plastics.

[0019] Optionally, the method for preparing the chitosan solution comprises the following steps: dispersing chitosan in an acetic acid solution, adding sodium alginate and hydroxyethyl cellulose, and stirring at 50-55° C. for 1-2 hours to obtain a chitosan solution.

[0020] By adopting the above technical scheme, chitosan is dissolved in acetic acid solution to form a transparent chitosan solution, sodium alginate and hydroxyethyl cellulose are added, sodium alginate and chitosan undergo ion crosslinking reaction to form a composite gel, which improves the mechanical properties and bonding properties of the composite gel, and the amino groups of chitosan and the hydroxyl groups of hydroxyethyl cellulose form chemical bonds to enhance the structural stability of the material, and improve the mechanical properties, thermal stability and chemical stability of the material. Chitosan, sodium alginate and hydroxyethyl cellulose cooperate with each other to improve the mechanical properties, viscosity and stability of the solution, and are subsequently sprayed on the surface of the mixture, which has good film-forming properties and viscosity, and helps to stabilize the performance of the mixture, and is subsequently applied to plastics to improve the corresponding properties of the plastics.

[0021] Optionally, the method for preparing the modified glass fiber comprises the following steps: (1) dispersing the glass fiber in a sodium hydroxide solution, stirring at a temperature of 70-75° C. for 1-2 hours, filtering, heating at 200-230° C. for 2-3 hours, and then dispersing in an aqueous solution of coupling agent KH570, stirring evenly, filtering, and obtaining pretreated glass fiber; (2) dispersing graphene in deionized water, adding sodium dodecylbenzene sulfonate, stirring at a temperature of 85-90° C. for 20-25 min, filtering, and drying to obtain pretreated graphene; (3) Dispersing the pretreated glass fiber in step (1) in deionized water, adding the pretreated graphene and modified lignin in step (2), stirring for 3-4 hours, and drying to obtain modified glass fiber.

[0022] By adopting the above technical solution, the sodium hydroxide solution erodes the surface of the glass fiber to a certain extent, making the surface of the glass fiber uneven, increasing the specific surface area of ​​the glass fiber, and increasing the roughness of the surface of the glass fiber, which helps to improve the mechanical bite between the glass fiber and the matrix material, and further enhances the interfacial bonding of the composite material. The glass fiber is calcined at 200-230°C to remove organic matter on the surface of the glass fiber, exposing more active sites, thereby improving the interfacial bonding between the glass fiber and the matrix material. Finally, it is dispersed in an aqueous solution of coupling agent KH570. KH570 can form chemical bonds on the surface of the glass fiber, and react with the silanol groups on the surface of the glass fiber through its silanol groups to form covalent bonds, thereby improving the mechanical properties of the composite material, such as tensile strength, flexural strength and impact resistance.

[0023] Graphene has extremely high strength and rigidity. Adding it to plastics can significantly improve the tensile strength, modulus and toughness of plastics, making the plastics have better mechanical properties while maintaining light weight. Sodium dodecylbenzene sulfonate is added. Sodium dodecylbenzene sulfonate has hydrophilic sodium sulfonate groups and hydrophobic dodecyl chains, which can be adsorbed on the surface of graphene to form a stable monolayer. This monolayer can prevent the aggregation caused by van der Waals forces between graphene sheets, thereby improving the dispersibility of graphene in aqueous media. The addition of sodium dodecylbenzene sulfonate enables graphene to form a stable aqueous suspension, which is convenient for subsequent processing and application.

[0024] Pretreated glass fiber and pretreated graphene are mixed, and graphene can be loaded on the surface of glass fiber to improve the tensile strength, elasticity and toughness of glass fiber. Modified lignin dispersed in deionized water has a certain viscosity, which can make graphene adhere to the surface of glass fiber, so that graphene can be stably loaded on the surface of glass fiber, which significantly improves the mechanical strength and wear resistance of glass fiber such as tensile strength, flexural strength and impact toughness, and subsequently improves the corresponding performance of plastics.

[0025] Optionally, the mass ratio of the glass fiber, graphene and modified lignin is 1g:50-60mg:0.3-0.6g.

[0026] By adopting the above technical scheme, the mass ratio of glass fiber, graphene and straw fiber is further limited within a certain range, the mechanical properties of glass fiber are improved, graphene can be loaded on the surface of glass fiber, and modified lignin makes graphene adhere to the surface of glass fiber. The glass fiber, graphene and modified lignin have a synergistic effect. Glass fiber has high strength and high modulus, graphene has extremely high strength and rigidity, and modified lignin can be used as an adhesive. The mixture of the three can significantly improve the mechanical strength and wear resistance of the composite material such as tensile strength, flexural strength and impact toughness, and can be subsequently applied to plastics to improve the corresponding performance of plastics.

[0027] Optionally, the preparation method of the modified lignin comprises the following steps: dispersing the lignin in hydrogen peroxide, stirring for 16-20 minutes, washing with water, and then dispersing in deionized water, adding montmorillonite and cellulose, stirring evenly, filtering, and obtaining the modified lignin.

[0028] By adopting the above technical scheme, lignin is surface treated with hydrogen peroxide, and hydrogen peroxide oxidizes the functional groups such as phenolic hydroxyl, methoxyl and side chain in the lignin molecule, thereby improving the roughness of lignin and helping lignin to mix with other substances. Montmorillonite has good mechanical properties, can be loaded on the surface of lignin, cooperate with lignin, improve the mechanical properties of lignin, and be subsequently applied to plastics to improve the tensile strength, flexural strength and impact toughness of plastics. The mixing of cellulose lignin can improve the tensile strength, flexural strength and impact toughness of composite materials, and the high crystallinity of cellulose and the cross-linking effect of lignin can form a stable network structure, thereby improving the rigidity and toughness of composite materials. Montmorillonite can be evenly dispersed in the cellulose matrix, forming a nano-scale reinforcing phase, thereby improving the rigidity and toughness of composite materials. Lignin, montmorillonite and cellulose are mixed to jointly improve the mechanical properties of the system.

[0029] Optionally, the coupling agent is a mixture of 3-acryloxypropylmethyldimethoxysilane and 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane.

[0030] By adopting the above technical solution, the coupling agent can enhance the interface bonding between the modified glass fiber, talcum powder and the PP / HDPE matrix, improve the dispersibility and compatibility of the filler in the plastic matrix, and improve the thermal stability of the composite material.

[0031] Preferably, the anti-aging agent is n-octadecyl β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and the antistatic agent is tetradecyltrimethylammonium hydrogen sulfate and / or dodecyltrimethylammonium hydrogen sulfate.

[0032] By adopting the above technical solutions, anti-aging agents can delay the performance degradation of PP / HDPE plastics caused by oxidation during processing and use, and extend the service life of plastic products. Antistatic agents can reduce the resistance of the plastic surface, reduce the accumulation of static charges, and prevent static discharge, thereby avoiding safety hazards such as fire and explosion caused by static electricity.

[0033] In the second aspect, the present application provides a method for preparing PP / HDPE plastic for automotive interior, comprising the following steps: mixing polypropylene, EPDM rubber, high-density polyethylene, modified walnut shell powder, maleic anhydride grafted polypropylene, anti-aging agent, nano-ceramic particles, coupling agent, modified glass fiber, antistatic agent, and talcum powder at a stirring rate of 300-400 r / min, a stirring temperature of 80-90°C, a stirring time of 3-6 min, and extruding and granulating to obtain PP / HDPE plastic for automotive interior.

[0034] By adopting the above technical scheme, the present application mixes the various raw material components, the production process is simple, the preparation efficiency is high, and PP / HDPE plastics for automotive interiors with excellent performance in all aspects are obtained, thereby improving the mechanical properties and wear resistance of the plastics.

[0035] In summary, this application has the following beneficial effects: 1. In the present application, polypropylene has good chemical stability and mechanical properties, enhances the rigidity of PP / HDPE blends, makes it not easy to deform when under pressure, improves the heat resistance of PP / HDPE blends, makes it still maintain good performance in high temperature environment, improves the impact resistance of PP / HDPE, makes it not easy to break when subjected to external force impact; high-density polyethylene has high strength, tolerance and tear resistance, enhances the mechanical properties and chemical stability of PP / HDPE blends, and reduces cracks caused by environmental stress.

[0036] 2. The modified walnut shell powder in this application has high hardness, good thermal stability and rigidity. It is added to PP / HDPE plastic to improve the hardness and wear resistance of the material, making it more durable during use, and improve the heat resistance of PP / HDPE plastic so that it can still maintain good performance in high temperature environment. It enhances the rigidity of PP / HDPE plastic and improves its bending strength, so that it is not easy to deform when under pressure.

[0037] 3. The modified glass fiber in the present application has good strength, wear resistance and toughness, and cooperates with the modified walnut shell powder and nano-ceramic particles to enhance the tensile strength, compressive strength, tear resistance and impact resistance of PP / HDPE plastics, making them more durable; the nano-ceramic particles can be loaded on the surface and pores of the modified walnut shell powder, improve the hardness, strength, good thermal stability and wear resistance of polypropylene, and can enhance the tensile strength, compressive strength and impact resistance of polypropylene. DETAILED DESCRIPTION

[0038] Preparation example of modified walnut shell powder Preparation Example 1-1 The preparation method of modified walnut shell powder comprises the following steps: (1) Grind 1.2 kg of walnut shells, disperse them in 1.9 L of deionized water, stir them at 85° C. for 15 min, add 0.8 L of 10% sodium hydroxide solution, continue stirring for 35 min, filter, and dry to obtain pretreated walnut shell powder; (2) dispersing the nano-silica in 1 L of a 30% by mass sulfuric acid solution, soaking for 30 min, washing with water, and filtering to obtain pretreated nano-silica; (3) Dispersing the pretreated walnut shell powder of step (1) in 2.5 L of deionized water, adding the pretreated nano-silica of step (2), stirring evenly, adding straw fiber filaments, stirring evenly, filtering, and drying to obtain a mixture, spraying 0.02 kg of chitosan solution on the surface of the mixture, and drying to obtain modified walnut shell powder.

[0039] The mass ratio of walnut shell, nano-silicon dioxide and straw fiber is 1:0.3:0.1.

[0040] The preparation method of chitosan solution comprises the following steps: dispersing 0.3 kg chitosan in 0.8 L acetic acid solution with a mass fraction of 25%, adding 0.1 kg sodium alginate and 0.09 kg hydroxyethyl cellulose, and stirring at 55° C. for 2 hours to obtain chitosan solution.

[0041] Preparation Example 1-2 The difference from Preparation Example 1-1 is that in step (2), no nano-silicon dioxide is added.

[0042] Preparation Example 1-3 The difference from Preparation Example 1-1 is that in step (3), no straw fiber is added.

[0043] Preparation Example 1-4 The difference from Preparation Example 1-1 is that in step (3), no chitosan solution is added.

[0044] Preparation Example 1-5 The difference from Preparation Example 1-1 is that the mass ratio of walnut shell, nano-silicon dioxide and straw fiber is 1:0.5:0.2.

[0045] Preparation Example 1-6 The difference from Preparation Example 1-1 is that the mass ratio of walnut shell, nano-silicon dioxide and straw fiber is 1:0.1:0.4.

[0046] Preparation Example 1-7 The difference from Preparation Example 1-1 is that no sodium alginate is added in the preparation method of the chitosan solution.

[0047] Preparation Example 1-8 The difference from Preparation Example 1-1 is that hydroxyethyl cellulose is not added in the preparation method of the chitosan solution.

[0048] Preparation example of modified glass fiber Preparation Example 2-1 The preparation method of modified glass fiber comprises the following steps: (1) 1.2 kg of glass fiber was dispersed in 2 L of 15% sodium hydroxide solution, stirred at 75° C. for 2 h, filtered, heated at 220° C. for 3 h, and then dispersed in 1.5 L of 0.2% coupling agent KH570 aqueous solution, stirred evenly, and filtered to obtain pretreated glass fiber; (2) dispersing graphene in 0.5 L of deionized water, adding 0.03 kg of sodium dodecylbenzene sulfonate, stirring at 90 ° C for 25 min, filtering, and drying to obtain pretreated graphene; (3) Dispersing the pretreated glass fiber in step (1) in 1.3 L of deionized water, adding the pretreated graphene and modified lignin in step (2), stirring for 4 h, and drying to obtain modified glass fiber.

[0049] The mass ratio of glass fiber, graphene and modified lignin is 1g:50mg:0.6g.

[0050] The preparation method of modified lignin comprises the following steps: dispersing 0.9 kg lignin in 1.1 L hydrogen peroxide, stirring for 20 min, washing with water, and then dispersing in 1.5 L deionized water, adding 0.2 kg montmorillonite and 0.05 kg cellulose, stirring evenly, filtering, and obtaining modified lignin.

[0051] Preparation Example 2-2 The difference from Preparation Example 2-1 is that in step (2), no graphene is added.

[0052] Preparation Example 2-3 The difference from Preparation Example 2-1 is that in step (3), no modified lignin is added.

[0053] Preparation Example 2-4 The difference from Preparation Example 2-1 is that the mass ratio of glass fiber, graphene and modified lignin is 1g:60mg:0.3g.

[0054] Preparation Example 2-5 The difference from Preparation Example 2-1 is that the mass ratio of glass fiber, graphene and modified lignin is 1g:30mg:0.9g.

[0055] Preparation Example 2-6 The difference from Preparation Example 2-1 is that montmorillonite is not added in the preparation method of the modified lignin.

[0056] Preparation Example 2-7 The difference from Preparation Example 2-1 is that no cellulose is added in the preparation method of the modified lignin. Example

[0057] Example 1 A PP / HDPE plastic for automobile interior decoration includes the following raw materials by weight: 80kg of polypropylene, 15kg of EPDM rubber, 30kg of high-density polyethylene, 25kg of modified walnut shell powder, 2kg of anti-aging agent, 2kg of maleic anhydride grafted polypropylene, 6kg of nano-ceramic particles, 1kg of coupling agent, 16kg of modified glass fiber, 0.3kg of antistatic agent and 10kg of talcum powder.

[0058] The coupling agent is prepared by mixing 3-acryloxypropylmethyldimethoxysilane and 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane in a mass ratio of 1:1.

[0059] The anti-aging agent is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and the antistatic agent is tetradecyltrimethylammonium hydrogen sulfate.

[0060] The preparation method of PP / HDPE plastic for automobile interior comprises the following steps: mixing polypropylene, EPDM rubber, high-density polyethylene, modified walnut shell powder, maleic anhydride grafted polypropylene, anti-aging agent, nano-ceramic particles, coupling agent, modified glass fiber, antistatic agent and talcum powder, with a stirring rate of 350 r / min, a stirring temperature of 85° C. and a stirring time of 6 min, and extruding and granulating to obtain PP / HDPE plastic for automobile interior; wherein the extrusion temperature in the extruder is 210° C.

[0061] The modified nano bamboo charcoal fiber was prepared according to Preparation Example 1-1, and the modified chitosan was prepared according to Preparation Example 2-1.

[0062] Example 2 A PP / HDPE plastic for automobile interior, which differs from Example 1 in that, measured by weight, it comprises the following raw materials: 90 kg of polypropylene, 18 kg of EPDM rubber, 35 kg of high-density polyethylene, 25 kg of modified walnut shell powder, 3 kg of anti-aging agent, 5 kg of maleic anhydride grafted polypropylene, 9 kg of nano-ceramic particles, 3 kg of coupling agent, 18 kg of modified glass fiber, 0.5 kg of antistatic agent, and 15 kg of talcum powder.

[0063] Example 3 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts the preparation example 1-2.

[0064] Example 4 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Example 1-3.

[0065] Example 5 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Examples 1-4.

[0066] Example 6 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Example 1-5.

[0067] Example 7 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Example 1-6.

[0068] Example 8 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Example 1-7.

[0069] Example 9 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder adopts Preparation Example 1-8.

[0070] Example 10 A PP / HDPE plastic for automobile interior, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-2.

[0071] Embodiment 11 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-3.

[0072] Example 12 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-4.

[0073] Embodiment 13 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-5.

[0074] Embodiment 14 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-6.

[0075] Embodiment 15 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber adopts Preparation Example 2-7.

[0076] Comparative Example Comparative Example 1 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that modified walnut shell powder is not added.

[0077] Comparative Example 2 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified walnut shell powder is replaced by an equal amount of walnut shell powder.

[0078] Comparative Example 3 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that modified glass fiber is not added.

[0079] Comparative Example 4 A PP / HDPE plastic for automobile interior decoration, which is different from Example 1 in that the modified glass fiber is replaced by an equal amount of glass fiber.

[0080] Performance testing The PP / HDPE plastics prepared in Examples 1-15 and Comparative Examples 1-4 were subjected to performance tests.

[0081] The tensile strength and elongation at break were tested with reference to GB / T1040.1-2006, the flexural strength and flexural modulus were tested with reference to GB / T9341-2008, and the cantilever beam notched impact strength was tested with reference to GB / T1043.1-2008. The wear resistance of PP / HDPE plastics for automotive interiors was tested with reference to GB3960-1983, and friction tests were conducted. The friction tests included two types of tests, one under dry friction conditions and the other under water lubrication conditions. The test results are shown in Table 1.

[0082] Table 1 Test data of embodiments and comparative examples Combining the examples and the data in Table 1, it can be seen that the PP / HDPE plastics for automotive interiors prepared in Examples 1-2, Example 6 and Example 12 have good mechanical properties and wear resistance. Among them, the tensile strength of Example 1 is 78 MPa, the elongation at break is 120%, the flexural strength is 91.2 MPa, the flexural modulus is 2978 MPa, and the cantilever beam notched impact strength is 38.3 KJ / m 2 The wear rate under dry friction conditions is 1.23×10 -6 mm 3 ﹒ N -1 ﹒ m -1 The wear rate under water lubrication conditions is 0.12×10 -6 mm 3 ﹒ N -1 ﹒ m -1 , indicating that the PP / HDPE plastic prepared in this application has good impact resistance, tensile strength and wear resistance. The various components cooperate with each other to jointly improve the mechanical strength and chemical stability of the plastic, and have good resistance to environmental stress cracking.

[0083] In the preparation method of the modified walnut shell powder in Example 3, no nano-silicon dioxide is added, in the preparation method of the modified walnut shell powder in Example 4, no straw fiber is added, and in the preparation method of the modified walnut shell powder in Example 5, no chitosan solution is added. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, and cantilever beam notched impact strength are all significantly reduced, and the wear rate under dry friction conditions and the wear rate under water lubrication conditions are both increased, indicating that nano-silicon dioxide has high hardness, good dispersibility, and excellent thermal stability, and can improve the tensile strength, impact resistance, wear resistance and scratch resistance of plastics. The straw fiber has high porosity, flexibility and tensile strength, which can improve the corresponding properties of plastics. The chitosan solution has certain viscosity, film-forming property, heat resistance and mechanical properties, which can improve the corresponding properties of plastics.

[0084] Example 7 changes the mass ratio of walnut shell, nano-silicon dioxide and straw fiber filaments. It can be seen from Table 1 that compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength and wear rate are better than those of Examples 3-4, but worse than those of Examples 1-2 and Example 6, indicating that nano-silicon dioxide can be loaded on the surface and pores of walnut powder, and walnut shell powder loaded with nano-silicon dioxide can be loaded on the surface and pores of straw fiber filaments. Walnut shell, nano-silicon dioxide and straw fiber filaments have a synergistic effect, which can be subsequently applied to plastics to improve the corresponding properties of plastics.

[0085] In the preparation methods of chitosan solutions of Examples 8-9, sodium alginate and hydroxyethyl cellulose are not added respectively. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength, and wear rate are significantly worse than those of Examples 1-2, but better than those of Example 5, indicating that chitosan, sodium alginate and hydroxyethyl cellulose cooperate with each other to improve the mechanical properties, viscosity and stability of the solution. The subsequent spraying on the surface of the mixture has good film-forming properties and viscosity, which helps to stabilize the performance of the mixture, and is subsequently applied to plastics to improve the corresponding properties of the plastics.

[0086] Graphene is not added in the preparation method of the modified glass fiber in Example 10, and modified lignin is not added in the preparation method of the modified glass fiber in Example 11. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, and cantilever beam notched impact strength are all significantly reduced, and the wear rate under dry friction conditions and the wear rate under water lubrication conditions are both increased, indicating that graphene has extremely high strength and rigidity, and adding it to plastics can significantly improve the tensile strength, modulus and toughness of plastics. The modified lignin dispersed in deionized water has a certain viscosity, which can make graphene adhere to the surface of the glass fiber, so that the graphene is stably loaded on the surface of the glass fiber, which significantly improves the mechanical strength and wear resistance of the glass fiber such as tensile strength, flexural strength and impact toughness, and subsequently improves the corresponding properties of the plastic.

[0087] Example 13 changes the mass ratio of glass fiber, graphene and modified lignin. It can be seen from Table 1 that compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength and wear rate are better than those of Example 10-11, but worse than those of Example 1-2 and Example 12, indicating that the glass fiber, graphene and modified lignin have a synergistic effect. The glass fiber has high strength and high modulus, the graphene has extremely high strength and rigidity, and the modified lignin can be used as an adhesive. The mixture of the three can significantly improve the mechanical strength and wear resistance of the composite material such as tensile strength, flexural strength and impact toughness, and can be subsequently applied to plastics to improve the corresponding properties of the plastics.

[0088] In the preparation methods of modified lignin in Examples 14-15, no montmorillonite or cellulose is added respectively. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength, and wear rate are significantly worse than those in Examples 1-2, but better than those in Example 11, indicating that montmorillonite has good mechanical properties and can be loaded on the surface of lignin and combined with lignin to improve the mechanical properties of lignin, and subsequently applied to plastics to improve the tensile strength, flexural strength and impact toughness of the plastics; the mixing of cellulose and lignin can improve the tensile strength, flexural strength and impact toughness of the composite material, and the high crystallinity of cellulose and the cross-linking effect of lignin can form a stable network structure, thereby improving the rigidity and toughness of the composite material.

[0089] Comparative Examples 1 and 3 do not add modified walnut shell powder and modified glass fiber, respectively. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength, and wear rate are significantly worse than those of Examples 1-2, indicating that the modified walnut shell powder has higher hardness, better thermal stability and rigidity, and is added to PP / HDPE plastic to improve the hardness and wear resistance of the material, making it more durable during use; the modified glass fiber has better strength, wear resistance and toughness, and cooperates with the modified walnut shell powder and nano-ceramic particles to enhance the tensile strength, compressive strength, tear resistance and impact resistance of the PP / HDPE plastic, making it more durable.

[0090] Comparative Example 2 and Comparative Example 4 are prepared by replacing the modified walnut shell powder with an equal amount of walnut shell powder and replacing the modified glass fiber with an equal amount of glass fiber, respectively. As can be seen from Table 1, compared with Example 1, the tensile strength, elongation at break, flexural strength, flexural modulus, cantilever beam notched impact strength, and wear rate are significantly worse than those of Examples 1-2, but better than Comparative Example 1 and Comparative Example 3, indicating that the modified walnut shell powder and glass fiber of the present application have good strength, toughness and wear resistance, thereby subsequently improving the corresponding properties of the plastic.

[0091] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A PP / HDPE plastic for automobile interior, characterized in that: The raw materials are as follows, measured by weight: 80-90 parts of polypropylene, 15-18 parts of EPDM rubber, 30-35 parts of high-density polyethylene, 25-28 parts of modified walnut shell powder, 2-3 parts of anti-aging agent, 2-5 parts of maleic anhydride grafted polypropylene, 6-9 parts of nano-ceramic particles, 1-3 parts of coupling agent, 16-18 parts of modified glass fiber, 0.3-0.5 parts of antistatic agent and 10-15 parts of talc.

2. The PP / HDPE plastic for automobile interior according to claim 1, characterized in that: The preparation method of the modified walnut shell powder comprises the following steps: (1) Grinding the walnut shells, dispersing them in deionized water, stirring them at 80-85° C. for 10-15 minutes, adding sodium hydroxide, continuing to stir for 30-35 minutes, filtering, and drying to obtain pretreated walnut shell powder; (2) dispersing nano-silica in a sulfuric acid solution, soaking for 25-30 minutes, washing with water, and filtering to obtain pretreated nano-silica; (3) Dispersing the pretreated walnut shell powder of step (1) in deionized water, adding the pretreated nano-silicon dioxide of step (2), stirring evenly, adding straw fiber filaments, stirring evenly, filtering, drying to obtain a mixture, spraying chitosan solution on the surface of the mixture, and drying to obtain modified walnut shell powder.

3. The PP / HDPE plastic for automobile interior decoration according to claim 2, characterized in that: The mass ratio of the walnut shell, nano silicon dioxide and straw fiber is 1:0.3-0.5:0.1-0.

2.

4. The PP / HDPE plastic for automobile interior according to claim 2, characterized in that: The method for preparing the chitosan solution comprises the following steps: dispersing chitosan in an acetic acid solution, adding sodium alginate and hydroxyethyl cellulose, and stirring at 50-55° C. for 1-2 hours to obtain the chitosan solution.

5. The PP / HDPE plastic for automobile interior decoration according to claim 1, characterized in that: The method for preparing the modified glass fiber comprises the following steps: (1) Dispersing the glass fiber in a sodium hydroxide solution, stirring at a temperature of 70-75°C for 1-2 hours, filtering, heating at 200-230°C for 2-3 hours, and then dispersing it in an aqueous solution of coupling agent KH570, stirring evenly, filtering, and obtaining pretreated glass fiber; (2) dispersing graphene in deionized water, adding sodium dodecylbenzene sulfonate, stirring at a temperature of 85-90° C. for 20-25 min, filtering, and drying to obtain pretreated graphene; (3) Dispersing the pretreated glass fiber in step (1) in deionized water, adding the pretreated graphene and modified lignin in step (2), stirring for 3-4 hours, and drying to obtain modified glass fiber.

6. The PP / HDPE plastic for automobile interior according to claim 5, characterized in that: The mass ratio of the glass fiber, graphene and modified lignin is 1g:50-60mg:0.3-0.6g.

7. The PP / HDPE plastic for automobile interior decoration according to claim 5, characterized in that: The preparation method of the modified lignin comprises the following steps: dispersing the lignin in hydrogen peroxide, stirring for 16-20 minutes, washing with water, and then dispersing in deionized water, adding montmorillonite and cellulose, stirring evenly, filtering, and obtaining the modified lignin.

8. The PP / HDPE plastic for automobile interior according to claim 1, characterized in that: The coupling agent is prepared by mixing 3-acryloxypropylmethyldimethoxysilane and 3-[(2,3)-epoxypropyloxy]propylmethyldimethoxysilane.

9. The PP / HDPE plastic for automobile interior decoration according to claim 1, characterized in that: The anti-aging agent is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, and the antistatic agent is tetradecyltrimethylammonium hydrogen sulfate and / or dodecyltrimethylammonium hydrogen sulfate.

10. The method for preparing PP / HDPE plastic for automobile interior according to claim 1, characterized in that: The method comprises the following steps: mixing polypropylene, EPDM rubber, high-density polyethylene, modified walnut shell powder, maleic anhydride grafted polypropylene, anti-aging agent, nano-ceramic particles, coupling agent, modified glass fiber, antistatic agent and talcum powder at a stirring rate of 300-400 r / min, a stirring temperature of 80-90° C., a stirring time of 3-6 minutes, and extruding and granulating to obtain PP / HDPE plastic for automobile interior decoration.

Citation Information

Patent Citations

  • Anti-ageing PP / HDPE (Polypropylene / High-Density Polyethylene) plastic for automobile interior and preparation method thereof

    CN102649855A

  • Anti-impact modified PP / HDPE (Polypropylene / High Density Polyethylene) plastics for automotive interior parts and preparation method thereof

    CN103059416A

  • Glass fiber reinforced antibacterial PP plastic masterbatch and preparation method thereof

    CN106188841A

  • Low VOC polypropylene composite material for automotive trim

    CN107082962A