High-strength regenerated polypropylene composite material and preparation method thereof
By preparing functionalized graphene in regenerated polypropylene materials and performing cross-linking reactions, the problem of degradation of mechanical properties of regenerated polypropylene materials is solved, significantly improving its mechanical properties, and expanding its application range and service life.
Patent Information
- Application Number
- CN202411265279.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The mechanical properties of recycled polypropylene materials have been reduced after multiple processing, which limits their application range in automobiles, home appliances and other fields, and is difficult to expand the recycling range.
By preparing a suspension in a toluene solvent, magnetic stirring and heating reflux, functional graphene is formed, and melt extruded with polypropylene in a twin-screw extruder to form, forming a Cross-linked mesh structure to improve the mechanical properties of the material.
It significantly improves the tensile strength, bending strength and impact strength of recycled polypropylene composite materials, expands its application field, enhances mechanical properties, and extends the service life of the material.
Smart Images

Figure BDA0005036949170000051 
Figure BDA0005036949170000061 
Figure BDA0005036949170000091
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer materials, and in particular to a high-strength recycled polypropylene composite material and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is one of the five general-purpose plastics. It is widely used in many fields such as automobiles, home appliances, electronic appliances, power tools, and medical treatment because of its good physical, chemical, mechanical and processing properties. However, a large amount of waste plastics have also been generated. In recent years, the world has also begun to respond to carbon neutrality policies. Therefore, the use of these waste plastics will become a future development theme. Since the source of recycled materials is generally the dismantling of scrap plastic parts, and obtained through cleaning and granulation, the recycled materials are degraded after multiple processing, which also leads to the addition of recycled materials. Products will affect the mechanical properties of the product, thereby affecting its further expansion in application areas. In order to expand the scope of recycling of recycled polypropylene materials, the present invention provides a high-strength recycled polypropylene composite material and a preparation method thereof. Summary of the invention
[0003] In view of the deficiencies in the prior art, the present invention provides a high-strength recycled polypropylene composite material and a preparation method thereof.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] The first aspect of the present invention relates to a recycled polypropylene composite material, comprising the following raw materials in parts by weight:
[0006] Polypropylene 6-74.5 parts, recycled polypropylene 10-50 parts, initiator A 0.01-1 parts, silane coupling agent B 1-5 parts, functionalized graphene 1-3 parts,
[0007] Wherein, the preparation method of the functionalized graphene comprises the following steps:
[0008] Putting graphene, silane coupling agent B, initiator B and PE powder in a toluene solvent in a mass ratio of (10-20) / (2-10) / (0.1-0.5) / (69.5-87.9) to prepare a suspension, and adding the total mass of graphene, silane coupling agent B, initiator B and PE powder to the toluene solvent in a ratio of 1 / (3-8);
[0009] The suspension is magnetically stirred and heated to reflux;
[0010] The suspension is separated into solid and liquid, cleaned and dried to obtain the functionalized graphene.
[0011] Optionally, the polypropylene is at least one of homopolypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer, and propylene-1-butene random block.
[0012] Optionally, the following auxiliary materials in parts by weight are also included:
[0013] 5 to 30 parts of inorganic filler, 2 to 15 parts of toughening agent, 0.5 to 2 parts of deodorant and 0.5 to 3 parts of processing aid.
[0014] Optionally, the processing aid is at least one of an antioxidant, a weathering agent, a lubricant, and a toner.
[0015] Optionally, the graphene particle size D50≤5um; the silane coupling agent A or B is at least one of a vinyl silane coupling agent or an allyl silane coupling agent; the initiator A or B is at least one of diisopropylbenzene peroxide (DCP), di-tert-butyl peroxide diisopropylbenzene (BIPB), and azobisisobutyronitrile (AIBN); and the PE powder is at least one of LDPE and HDPE.
[0016] Optionally, the recycled polypropylene is at least one of household appliance housing decomposition granulation material, battery shell crushing granulation material, and ton bag crushing granulation material.
[0017] Optionally, the PE powder is at least one of LDPE and HDPE.
[0018] Optionally, the inorganic filler is at least one of talc, whiskers, mica, wollastonite and calcium carbonate.
[0019] Optionally, the toughening agent is at least one of POE, LDPE, HDPE, SEBS, and EPDM.
[0020] Optionally, the deodorant is porous silicate.
[0021] A second aspect of the present invention relates to a method for preparing a polypropylene composite material, comprising the following steps:
[0022] Putting graphene, silane coupling agent B, initiator B, and PE powder in a toluene solvent in a mass ratio of (10-20) / (2-10) / (0.1-0.5) / (69.5-87.9) to prepare a suspension, wherein the total mass ratio of the added graphene, silane coupling agent B, initiator B, and PE powder to the toluene solvent is 1 / (3-8);
[0023] The suspension is magnetically stirred and heated to reflux;
[0024] The suspension is separated into solid and liquid, cleaned and dried to obtain functionalized graphene;
[0025] 6-74.5 parts by weight of polypropylene, 10-50 parts by weight of recycled polypropylene, 1-3 parts by weight of functionalized graphene, 1-5 parts by weight of silane coupling agent A, and 0.01-1 parts by weight of initiator A are uniformly mixed, and the polypropylene composite material is obtained through melting, extrusion, and cooling.
[0026] Furthermore, the extrusion process is carried out in a twin-screw extruder, which is divided into ten zones from the feed port to the die head, with temperatures ranging from 160 to 210° C.; the speed of the extruder is 300 to 500 rpm / min, double vacuum, and the vacuum degree is -0.07 to -0.03 MPa.
[0027] Beneficial effects of the present invention:
[0028] (1) The present invention utilizes PE, a silane coupling agent, and an initiator to perform surface treatment on graphene under certain conditions to obtain functionalized graphene powder, which is formed by a silane grafting and cross-linking reaction between active groups such as hydroxyl groups on the graphene surface and PE molecular chains, thereby not only improving the compatibility of graphene with polypropylene resin, but also improving the dispersibility of graphene.
[0029] (2) In the twin-screw extrusion granulation process, organic silane is used as a coupling agent and melt extrusion is carried out in the presence of a free radical initiator. The PP macromolecular free radical opens the double bonds on the silane molecular chain and grafts the unsaturated silane onto the PP chain. At the same time, the alkoxy groups of the grafted PP are hydrolyzed to produce hydroxyl groups, and then the silanol is dehydrated to form Si-O-Si bonds, thereby cross-linking the PP. In this process, the PE molecular chains grafted on the surface of the functionalized graphene also participate in the cross-linking reaction, so that the graphene is evenly grafted and distributed in the composite material system, forming a cross-linked network structure, which greatly improves the mechanical properties of the recycled polypropylene composite material. DETAILED DESCRIPTION
[0030] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0031] Unless otherwise specified, the raw materials and reagents used in the examples of the present invention are conventionally purchased raw materials and reagents.
[0032] Polypropylene, grade M60RHC, Zhenhai Refining and Chemical;
[0033] Recycled polypropylene, battery shell material, Jiangxi GreenMe;
[0034] Talc, 1250 mesh talc 90-20-A, Guangxi Longsheng Huamei Talc;
[0035] Toughener, POE, brand LC565, LG Chemical;
[0036] Graphene, brand NO-C-068-1, Shanghai Naionan Technology Co., Ltd.;
[0037] Porous silicate, brand JH-200A, average pore size 5nm, Ningbo Jiahe New Materials;
[0038] Other processing aids are commercially available conventional additives;
[0039] Silane coupling agent, vinyl triethoxysilane, brand KH-151, Hangzhou Jessica Chemical Co., Ltd.
[0040] Initiator, DCP, Aksu.
[0041] Regarding the initiator, it should be noted that, although in the content of the invention, for the sake of clear description and definition, the initiator and the silane coupling agent are distinguished by initiator A and initiator B, and silane coupling agent A and silane coupling agent B (used for the preliminary preparation of functionalized graphene, and used for the preparation of polypropylene composite materials), in actual implementation, the initiator A and the initiator B, and the silane coupling agent A and the silane coupling agent B, may use the same components or different components.
[0042] The preparation process of a high-strength recycled polypropylene composite material is as follows:
[0043] S1. Put graphene, silane coupling agent, initiator DCP and PE powder in a toluene solvent in a mass ratio of 15 / 3 / 0.2 / 81.8 to prepare a suspension, wherein the total mass of the added graphene, silane coupling agent, initiator DCP and PE powder and the solid-liquid ratio of the toluene solvent is 1 / 5; and start magnetic stirring and heating reflux for 2h; finally, put the prepared mixed suspension in a solid-liquid separation device, cool, filter, and wash it with ethanol and clean water, dry, grind it to prepare functionalized graphene composite material powder;
[0044] S2. Polypropylene, recycled polypropylene, talcum powder, toughening agent POE, deodorant, functionalized graphene, silane coupling agent, initiator DCP, antioxidant 1010, antioxidant 168, lubricant calcium stearate, black masterbatch, etc. are mixed evenly in proportion, and placed in a twin-screw extruder for melting, extrusion, cooling, and granulation to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0045] The specific formulas of Examples 1 to 5 are shown in Table 1.
[0046] Table 1
[0047]
[0048]
[0049] Comparative Example 1
[0050] 36 parts of polypropylene, 30 parts of recycled polypropylene, 15 parts of talc, 10 parts of toughening agent POE, 1 part of deodorant, 3 parts of graphene, 3 parts of silane coupling agent, 0.2 parts of initiator DCP, 0.2 parts of antioxidant 1010, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch are mixed evenly in proportion, and placed in a twin-screw extruder for melting, extrusion, cooling, and granulation to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0051] Comparative Example 2
[0052] S1. Put graphene, initiator DCP and PE powder in a toluene solvent in a mass ratio of 15 / 0.2 / 84.8 to prepare a suspension, wherein the total mass of the added graphene, initiator DCP and PE powder and the solid-liquid ratio of the toluene solvent is 1 / 5; and start magnetic stirring and heating reflux for 2h; finally, put the prepared mixed suspension in a solid-liquid separation device, cool, filter, and wash it with ethanol and clean water, dry, and grind it to prepare a surface-modified graphene composite material powder;
[0053] S2, 36 parts of polypropylene, 30 parts of recycled polypropylene, 15 parts of talc, 10 parts of toughening agent POE, 1 part of deodorant, 3 parts of functionalized graphene, 3 parts of silane coupling agent, 0.2 parts of initiator DCP, 0.2 parts of antioxidant 1010, 0.3 parts of lubricant calcium stearate, 1 part of black masterbatch are mixed evenly in proportion, and placed in a twin-screw extruder, melted, extruded, cooled, and granulated to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160℃, 210℃, 210℃, 210℃, 200℃, 200℃, 200℃, 200℃, 210℃, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0054] Comparative Example 3
[0055] S1. Put graphene, silane coupling agent and PE powder in a toluene solvent in a mass ratio of 15 / 3 / 82 to prepare a suspension, wherein the total mass of the added graphene, silane coupling agent and PE powder and the solid-liquid ratio of the toluene solvent is 1 / 5; and start magnetic stirring and heating reflux for 2h; finally, put the prepared mixed suspension in a solid-liquid separation device, cool, filter, and wash it with ethanol and clean water, dry, and grind it to prepare a surface-modified graphene composite material powder;
[0056] S2, polypropylene 36 powder, 30 parts of recycled polypropylene, 15 parts of talcum powder, 10 parts of toughening agent POE, 1 part of deodorant, 3 parts of functionalized graphene, 3 parts of silane coupling agent, 0.2 parts of initiator DCP, 0.2 parts of antioxidant 1010, 0.3 parts of lubricant calcium stearate, 1 part of black masterbatch are mixed evenly in proportion, and placed in a twin-screw extruder, melted, extruded, cooled, and granulated to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160℃, 210℃, 210℃, 210℃, 200℃, 200℃, 200℃, 200℃, 210℃, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0057] Comparative Example 4
[0058] S1. Graphene, silane coupling agent, initiator DCP, and PE powder are placed in a toluene solvent in a mass ratio of 15 / 3 / 0.2 / 81.8 to prepare a suspension, wherein the total mass of the added graphene, silane coupling agent, initiator DCP, and PE powder and the solid-liquid ratio of the toluene solvent are 1 / 5; and magnetic stirring and heating reflux are turned on for 2 hours; finally, the prepared mixed suspension is placed in a solid-liquid separation device, cooled, filtered, and washed with ethanol and clean water, dried, and ground to prepare a surface-modified graphene composite material powder;
[0059] S2. 36 parts of polypropylene, 30 parts of recycled polypropylene, 15 parts of talc, 10 parts of toughening agent POE, 1 part of deodorant, 3 parts of functionalized graphene, 3 parts of silane coupling agent, 0.2 parts of antioxidant 1010, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch are mixed evenly in proportion, and placed in a twin-screw extruder for melting, extrusion, cooling, and granulation to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160°C, 210°C, 210°C, 210°C, 200°C, 200°C, 200°C, 200°C, 210°C, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0060] Comparative Example 5
[0061] S1. Put graphene, silane coupling agent, initiator and PE powder in a toluene solvent in a mass ratio of 15 / 3 / 0.2 / 81.8 to prepare a suspension, wherein the total mass of the added graphene, silane coupling agent, initiator DCP and PE powder and the solid-liquid ratio of the toluene solvent is 1 / 5; and start magnetic stirring and heating reflux for 2h; finally, put the prepared mixed suspension in a solid-liquid separation device, cool, filter, and wash it with ethanol and clean water, dry, and grind it to prepare a surface-modified graphene composite material powder;
[0062] S2, 36 parts of polypropylene, 30 parts of recycled polypropylene, 15 parts of talcum powder, 10 parts of toughening agent POE, 1 part of deodorant, 3 parts of functionalized graphene, 0.2 parts of initiator DCP, 0.2 parts of antioxidant 1010, 0.3 parts of lubricant calcium stearate, and 1 part of black masterbatch are mixed evenly in proportion, and placed in a twin-screw extruder, melted, extruded, cooled, and granulated to obtain a high-strength recycled polypropylene composite material. The extruder is divided into ten zones from the feed port to the die head, and the temperatures of zones 1 to 10 are 160℃, 210℃, 210℃, 210℃, 200℃, 200℃, 200℃, 200℃, 210℃, respectively; the main engine speed is 400rpm / min, double vacuum, and the vacuum degree is -0.08MPa.
[0063] The recycled polypropylene composite materials obtained in Examples 1 to 5 and Comparative Examples 1 to 5 were tested for tensile strength, flexural strength, flexural modulus, notched impact strength, etc. It is worth noting that these tests are test methods familiar to those skilled in the art, and the specific test methods are not described here. The test results are shown in Table 2 below:
[0064] Table 2
[0065]
[0066] From the data in Table 2 above, it can be seen that the functionalized graphene prepared in a specific manner is cross-linked with the polypropylene system and the polypropylene itself is self-crosslinked, and the prepared recycled polypropylene composite material has excellent tensile strength, flexural strength, flexural modulus, impact strength and other performance indicators; from Example 3 and Comparative Example 1 and Comparative Example 2, it can be seen that when the functionalized graphene prepared in a specific manner is not added, the mechanical properties of the recycled polypropylene composite material finally prepared are significantly reduced; at the same time, according to Example 3 and Comparative Example 4 and Comparative Example 5, it can be seen that during the melt extrusion process, if the polypropylene resins and the polypropylene resins and the functionalized graphene cannot produce sufficient cross-linking reactions to form a network structure, the mechanical strength of the composite material cannot achieve better performance. According to the above summary, compared with the comparative example, the present invention significantly improves the mechanical properties of the recycled polypropylene composite material system. Therefore, the recycled polypropylene composite material prepared by the present invention can improve its performance range according to customer needs.
[0067] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0068] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A recycled polypropylene composite material, characterized in that: It includes the following raw materials in parts by weight: Polypropylene 6-74.5 parts, recycled polypropylene 10-50 parts, initiator A 0.01-1 parts, silane coupling agent A 1-5 parts, 1-3 parts of functionalized graphene, Wherein, the preparation method of the functionalized graphene comprises the following steps: Putting graphene, silane coupling agent B, initiator B and PE powder in a toluene solvent in a mass ratio of (10-20) / (2-10) / (0.1-0.5) / (69.5-87.9) to prepare a suspension, and adding graphene, silane coupling agent B, initiator B and PE powder in a total mass ratio of 1 / (3-8) to the toluene solvent; The suspension is magnetically stirred and heated to reflux; Then, the functionalized graphene is obtained through solid-liquid separation, washing and drying.
2. The polypropylene composite material according to claim 1, characterized in that: The polypropylene is at least one of homopolypropylene, propylene-ethylene block copolymer, propylene-ethylene random copolymer and propylene-1-butene random block.
3. The polypropylene composite material according to claim 1, characterized in that: The following auxiliary materials are also included: 5 to 30 parts of inorganic filler, 2 to 15 parts of toughening agent, 0.5 to 2 parts of deodorant and 0.5 to 3 parts of processing aid.
4. The high-strength recycled polypropylene composite material according to claim 3, characterized in that: The processing aid is at least one of an antioxidant, a weathering agent, a lubricant, and a toner.
5. The polypropylene composite material according to claim 1, characterized in that: The graphene particle size D50≤5um; the silane coupling agent A and the silane coupling agent B are selected from at least one of a vinyl silane coupling agent or an allyl silane coupling agent; the initiator A and the initiator B are selected from at least one of diisopropylbenzene peroxide, di-tert-butyl diisopropylbenzene peroxide, and azobisisobutyronitrile.
6. The polypropylene composite material according to claim 1, characterized in that: The PE powder is at least one of LDPE and HDPE.
7. The polypropylene composite material according to claim 3, characterized in that: The inorganic filler is at least one of talc, whisker, mica, wollastonite and calcium carbonate.
8. The polypropylene composite material according to claim 3, characterized in that: The toughening agent is at least one of POE, LDPE, HDPE, SEBS and EPDM.
9. The polypropylene composite material according to claim 3, characterized in that: The deodorant is porous silicate.
10. A method for preparing a polypropylene composite material, characterized in that: The following steps are involved: Putting graphene, silane coupling agent B, initiator B, and PE powder in a toluene solvent in a mass ratio of (10-20) / (2-10) / (0.1-0.5) / (69.5-87.9) to prepare a suspension, wherein the total mass ratio of the added graphene, silane coupling agent B, initiator B, and PE powder to the toluene solvent is 1 / (3-8); The suspension is magnetically stirred and heated to reflux; Then, functionalized graphene is obtained through solid-liquid separation, washing and drying; 6-74.5 parts by weight of polypropylene, 10-50 parts by weight of recycled polypropylene, 1-3 parts by weight of functionalized graphene, 1-5 parts by weight of silane coupling agent A, and 0.01-1 part by weight of initiator A are uniformly mixed, and the polypropylene composite material is obtained through melting, extrusion, and cooling.
Citation Information
Patent Citations
Polystyrene radical bamboo and plastic cabinet board modified by graphene oxide-grafted metallocene polyethylene compatibilizer and production method of polystyrene bamboo and plastic cabinet board
CN106084842A
Low-smell regenerated polypropylene composite material as internal and external trims of automobiles and preparation method of low-smell regenerated polypropylene composite material
CN108148281A
Carbon fiber reinforced polypropylene composite material and preparation method thereof
CN110885493A
Lightweight graphene composite material composition, lightweight graphene composite material and preparation method for lightweight graphene composite material
CN111087674A
Preparation method of micro-crosslinking antistatic graphene-based polypropylene composite material
CN112457571A