Closed-cell structure rubber and preparation method thereof, and protective adhesive tape and preparation method and application thereof

By adding specific components to butyl rubber to form a closed-cell structure and preparing multi-layer protective tape, it solves the problem that traditional materials are difficult to meet the airtightness, mechanical properties and physical properties of lightweight and high protection performance in the aerospace field. It has achieved improvements in structural strength and airtightness, and is suitable for protective clothing, aerospace and other fields.

CN118931056APending Publication Date: 2024-11-12CHEMCHINA SHUGUANG RUBBER IND RES&DESIGN INST C
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411218546.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional materials are difficult to meet the needs of lightweight and high protection performance in the fields of aerospace, while having airtightness, mechanical properties and physical properties.

Method used

By adding foaming agent, foaming additive, reinforcement filler, stearic acid, zinc oxide, sulfur, protective wax, anti-aging agent and accelerator to the butyl rubber, a closed-cell structure rubber is formed and protective tape is prepared. Combining multi-layer vulcanization technology with adhesive layer, skeleton layer and surface adhesive layer, the comprehensive performance of structural strength, airtightness and lightweight is achieved.

Benefits of technology

It has achieved improvements in the structural strength and airtightness of rubber, reduced weight, and improved the comprehensive performance of protective tape. It is suitable for protective clothing, aerospace and transportation fields, providing effective protection performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931056A_ABST
    Figure CN118931056A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of material synthesis, and particularly relates to closed-cell structure rubber and a preparation method thereof as well as a protective adhesive tape and a preparation method and application thereof. According to the closed-cell structure rubber provided by the invention, through the closed-cell structure, the self weight is effectively reduced, the overall load is reduced, the air tightness is good, meanwhile, the structural strength of the rubber can be maintained or even improved, and the comprehensive performance is excellent. The foaming agent is added into the rubber, so that closed-cell foaming is formed in the rubber, the unit weight of the rubber is effectively reduced, the overall load is reduced, and meanwhile, the structural strength and the protective performance of the rubber are maintained and even improved. The protective adhesive tape provided by the invention adopts the closed-cell structure rubber, has the characteristics of good structural strength, high protective performance and light weight, and is wide in application range. The protective adhesive tape provided by the invention is good in performance, can be widely applied to the fields of protective clothing, aerospace or transportation and the like, and provides effective protection for various protective scenes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of material synthesis, and in particular relates to a closed-cell structure rubber and a preparation method thereof, and a protective adhesive tape and a preparation method and application thereof. Background Art

[0002] As a highly elastic material, butyl rubber is a linear polymer with isobutylene as the main body and a small amount of isoprene bonded end to end. It is a saturated non-polar elastomer with excellent aging resistance and physical properties. The macromolecular chain has a large number of methyl substituents. The large number of substituents causes great steric hindrance, making it difficult for the molecular chain to move, which can effectively prevent gas molecules from penetrating and has excellent air tightness.

[0003] With the development of industry and materials science, the demand for high-performance protective materials is growing. Especially in scenarios where both lightweight and high protective performance need to be considered, such as aerospace and other fields, the air tightness, mechanical properties and physical properties of traditional materials are often difficult to meet the requirements. Summary of the invention

[0004] The purpose of the present invention is to provide a closed-cell structure rubber and a preparation method thereof, and a protective tape and a preparation method and application thereof. The closed-cell structure rubber provided by the present invention has the characteristics of good structural strength, good air tightness and light weight.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The invention provides a closed-cell structure rubber, which is prepared from the following raw materials, measured by weight: 100 parts of rubber, 5 to 8 parts of foaming agent, 2 to 4 parts of foaming aid, 10 to 20 parts of reinforcing filler, 1 to 2 parts of stearic acid, 2 to 5 parts of zinc oxide, 3 to 5 parts of sulfur, 1.5 to 2 parts of protective wax, 3 to 8 parts of antioxidant, and 0.8 to 2 parts of accelerator.

[0007] Preferably, the foaming agent is an organic foaming agent.

[0008] Preferably, the organic foaming agent includes one or more of azo compounds and sulfonylhydrazide compounds.

[0009] Preferably, the rubber includes one or more of butyl rubber, chlorinated butyl rubber and brominated butyl rubber.

[0010] The present invention also provides a method for preparing the closed-cell structure rubber described in the above scheme, comprising the following steps:

[0011] The rubber, foaming agent, foaming aid, reinforcing filler, stearic acid, zinc oxide, sulfur, protective wax, antioxidant and accelerator are mixed and vulcanized to obtain closed-cell structure rubber.

[0012] Preferably, the vulcanization conditions are: heating from 100° C. to 140-145° C. and keeping warm, the heating time is 60 min, and the keeping time is 60-80 min.

[0013] The present invention also provides a protective tape, comprising an adhesive layer, a skeleton layer arranged on the side of the adhesive layer, and a surface adhesive layer arranged on the other side of the adhesive layer; the surface adhesive layer is the closed-cell structure rubber described in the above scheme or the closed-cell structure rubber obtained by the preparation method described in the above scheme.

[0014] Preferably, the thickness ratio of the surface adhesive layer to the skeleton layer is 20-25:18-20; the thickness ratio of the surface adhesive layer to the adhesive layer is 20-25:1-2.

[0015] The present invention also provides a method for preparing the protective tape described in the above scheme, comprising the following steps:

[0016] The surface of one side of the skeleton layer is coated with the raw material mixture of the adhesive layer, and then the surface adhesive layer is coated with the raw material mixture of the surface adhesive layer to obtain a multilayer body, and the multilayer body is vulcanized to obtain the protective tape.

[0017] The present invention also provides the use of the protective tape described in the above scheme or the protective tape obtained by the preparation method described in the above scheme in the fields of protective clothing, aerospace or transportation.

[0018] The invention provides a closed-cell structure rubber. The closed-cell structure rubber provided by the invention can effectively reduce its own weight and overall load through the closed-cell structure, while maintaining or even improving the structural strength of the rubber, having good air tightness and excellent comprehensive performance.

[0019] The present invention also provides a method for preparing the closed-cell structure rubber described in the above scheme. The present invention adds a foaming agent to the rubber to form closed-cell foaming, which effectively reduces the unit weight of the rubber, reduces the overall load, has good air tightness, and maintains or even improves the structural strength of the rubber.

[0020] The present invention also provides a protective tape. The protective tape provided by the present invention adopts the closed-cell structure rubber described in the above scheme, and has the characteristics of good structural strength, high protective performance and light weight, and has a wide range of applications.

[0021] The present invention also provides a method for preparing the protective adhesive tape described in the above scheme. The preparation method provided by the present invention has simple steps, convenient operation and good feasibility.

[0022] The present invention also provides the use of the protective tape described in the above scheme or the protective tape obtained by the preparation method described in the above scheme in the field of protective clothing, aerospace or transportation. The protective tape provided by the present invention has good performance and can be widely used in the fields of protective clothing, aerospace or transportation, providing effective protection for various protection scenarios. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0024] Figure 1 A schematic diagram of the cross-sectional structure of the protective tape provided by the present invention;

[0025] Reference numerals: 1 is a surface adhesive layer, 2 is an adhesive layer, and 3 is a skeleton layer. DETAILED DESCRIPTION

[0026] The invention provides a closed-cell structure rubber, which is prepared from the following raw materials, measured by weight: 100 parts of rubber, 5 to 8 parts of foaming agent, 2 to 4 parts of foaming aid, 10 to 20 parts of reinforcing filler, 1 to 2 parts of stearic acid, 2 to 5 parts of zinc oxide, 3 to 5 parts of sulfur, 1.5 to 2 parts of protective wax, 3 to 8 parts of antioxidant, and 0.8 to 2 parts of accelerator.

[0027] The raw material of the closed-cell structure rubber provided by the present invention includes 100 parts of rubber. In the present invention, the rubber preferably includes one or more of butyl rubber, chlorinated butyl rubber and brominated butyl rubber. The above three rubbers in the present invention all have extremely low air permeability, that is, they have the same chemical penetration resistance.

[0028] The raw materials of the closed-cell structure rubber provided by the present invention include 5 to 8 parts of a foaming agent, preferably 6 to 7 parts, and more preferably 6.5 parts.

[0029] In the present invention, the foaming agent is preferably an organic foaming agent; the organic foaming agent preferably includes one or more of azo compounds and sulfonylhydrazide compounds; the azo compound is preferably diethyl azodicarboxylate; the sulfonylhydrazide compounds preferably include one or more of benzenesulfonylhydrazide and p-toluenesulfonylhydrazide. The above-mentioned organic foaming agent in the present invention is composed of elements such as carbon, hydrogen, oxygen and nitrogen, has a specific molecular structure and active groups, and has good compatibility with the polymer matrix. These characteristics enable it to form a stable and uniform closed-cell structure when mixed with rubber.

[0030] The raw materials of the closed-cell structure rubber provided by the present invention include 2 to 4 parts of a foaming aid, preferably 2.5 to 3.5 parts, and more preferably 3 parts.

[0031] In the present invention, the foaming aid is preferably zinc stearate. The foaming aid in the present invention can adjust the decomposition temperature and decomposition speed of the foaming agent during the foaming process, stabilize the foam structure, and improve the quality of the foamed body.

[0032] The raw materials of the closed-cell structure rubber provided by the present invention include 10 to 20 parts of reinforcing filler, preferably 12 to 18 parts, and more preferably 14 to 16 parts.

[0033] In the present invention, the reinforcing filler is preferably white carbon black. White carbon black has a significant reinforcing effect in rubber and can improve the physical and mechanical properties of rubber.

[0034] The raw materials of the closed-cell structure rubber provided by the present invention include 1 to 2 parts of stearic acid, preferably 1.2 to 1.8 parts, and more preferably 1.4 to 1.6 parts.

[0035] The raw materials of the closed-cell structure rubber provided by the present invention include 2 to 5 parts of zinc oxide, preferably 3 to 4 parts, and more preferably 3.5 parts.

[0036] The raw materials of the closed-cell structure rubber provided by the present invention include 3 to 5 parts of sulfur, preferably 3.5 to 4.5 parts, and more preferably 4 parts.

[0037] The raw materials of the closed-cell structure rubber provided by the present invention include 1.5 to 2 parts of protective wax, preferably 1.6 to 1.9 parts, and more preferably 1.7 to 1.8 parts.

[0038] In the present invention, the protective wax preferably includes one or more of paraffin wax and microcrystalline wax.

[0039] The raw materials of the closed-cell structure rubber provided by the present invention include 3 to 8 parts of antioxidant, preferably 4 to 7 parts, more preferably 5 to 6 parts.

[0040] In the present invention, the antioxidant preferably includes one or two of antioxidant TMQ and antioxidant 4426, more preferably antioxidant TMQ and antioxidant 4426; when the antioxidant is antioxidant TMQ and antioxidant 4426, the mass ratio of antioxidant TMQ and antioxidant 4426 is preferably 1-3:2-5, more preferably 1.5-2.5:3-4, and further preferably 2:3.5.

[0041] The raw materials of the closed-cell structure rubber provided by the present invention include 0.8 to 2 parts of accelerator, preferably 1 to 1.6 parts, and more preferably 1.2 to 1.4 parts.

[0042] In the present invention, the promoter preferably includes one or two of promoter DM and promoter TMTD, more preferably promoter DM and promoter TMTD; when the promoter is promoter DM and promoter TMTD, the mass ratio of promoter DM and promoter TMTD is preferably 0.3-1:0.5-1, more preferably 0.5-0.8:0.6-0.8, and further preferably 0.6-0.7:0.7.

[0043] The present invention also provides a method for preparing the closed-cell structure rubber described in the above scheme, comprising the following steps:

[0044] The rubber, foaming agent, foaming aid, reinforcing filler, stearic acid, zinc oxide, sulfur, protective wax, antioxidant and accelerator are mixed and vulcanized to obtain closed-cell structure rubber.

[0045] In the present invention, the vulcanization equipment is preferably a vulcanization tank; the vulcanization conditions are preferably: heating from 100°C to 140-145°C and keeping warm, the heating time is 60 minutes, and the keeping time is 60-80 minutes.

[0046] In the present invention, the insulation time is more preferably 60 to 75 minutes, and further preferably 65 to 70 minutes.

[0047] The present invention also provides a protective tape, comprising an adhesive layer, a skeleton layer arranged on the side of the adhesive layer, and a surface adhesive layer arranged on the other side of the adhesive layer; the surface adhesive layer is the closed-cell structure rubber described in the above scheme or the closed-cell structure rubber obtained by the preparation method described in the above scheme.

[0048] The protective tape provided by the present invention comprises an adhesive layer; the adhesive layer is preferably a chloroprene rubber adhesive layer; the chloroprene rubber adhesive layer is prepared from the following raw materials in terms of mass fractions:

[0049] 100 parts of chloroprene rubber, 1 part of stearic acid, 3 parts of magnesium oxide, 5 parts of zinc oxide, 20 parts of white carbon black, 2 parts of adhesive RE, 1.5 parts of accelerator H, 1 part of accelerator TMTD, 1 part of accelerator DM and 1.5 parts of sulfur. The chloroprene rubber adhesive layer in the present invention is compounded by adding chloroprene rubber to a meta-acetylene adhesive system adhesive, and has high bonding strength with nylon skeleton materials.

[0050] The protective tape provided by the present invention comprises a skeleton layer arranged on the side of the adhesive layer; the skeleton layer is preferably a nylon skeleton layer; the material of the nylon skeleton layer is preferably 507 nylon silk plain weave silk. The present invention adopts 507 nylon silk plain weave silk as synthetic fiber, which has excellent properties such as ultra-high strength, high modulus, high temperature resistance, acid and alkali resistance, light weight, anti-aging and long life cycle.

[0051] The protective tape provided by the present invention comprises a surface adhesive layer arranged on the other side of the adhesive layer. The present invention utilizes the surface adhesive layer to protect the object to be protected by the protective tape.

[0052] In the present invention, the thickness ratio of the surface rubber layer to the skeleton layer is preferably 20-25:18-20, more preferably 21-24:18.5-19.5, and further preferably 22-23:19.

[0053] In the present invention, the thickness ratio of the surface rubber layer to the adhesive layer is preferably 20-25:1-2, more preferably 21-24:1.2-1.8, and further preferably 22-23:1.4-1.6.

[0054] In the present invention, the total thickness of the protective tape is preferably 0.40 to 0.45 mm, more preferably 0.42 to 0.43 mm.

[0055] The present invention also provides a method for preparing the protective tape described in the above scheme, comprising the following steps:

[0056] The surface of one side of the skeleton layer is coated with the raw material mixture of the adhesive layer, and then the surface adhesive layer is coated with the raw material mixture of the surface adhesive layer to obtain a multilayer body, and the multilayer body is vulcanized to obtain the protective tape.

[0057] In the present invention, the raw material mixture of the adhesive layer is preferably: the raw material mixture of the adhesive layer is coated on one side surface of the skeleton layer; the raw material mixture of the covering rubber layer is preferably: the raw material mixture of the surface rubber layer is coated on one side surface of the adhesive layer.

[0058] In the present invention, the vulcanization equipment is preferably a vulcanization tank; the vulcanization conditions are preferably: heating from 100°C to 140°C for 60 minutes, and then heating from 140°C to 145°C for 60 to 80 minutes.

[0059] The present invention also provides the use of the protective tape described in the above scheme or the protective tape obtained by the preparation method described in the above scheme in the fields of protective clothing, aerospace or transportation.

[0060] The protective tape provided by the present invention has excellent performance and can be widely used in protective clothing, aerospace, transportation and other fields to provide effective protection for various protection scenarios.

[0061] In order to further illustrate the present invention, the scheme of the present invention is described in detail below in conjunction with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0062] Example

[0063] The cross-sectional structure of the protective tape prepared in this embodiment is as follows: Figure 1 As shown, the steps of the preparation method are as follows:

[0064] A chloroprene rubber adhesive is coated on a nylon skeleton material 3 to obtain a chloroprene rubber adhesive layer 2, and then a raw material mixture of a surface rubber layer 1 is coated on the chloroprene rubber adhesive layer 2, and vulcanized in a vulcanizer. The vulcanization conditions are: 100°C to 140°C for 60 min, 140°C to 145°C for 60 min, and a total of 120 min to obtain a protective tape.

[0065] The chloroprene rubber adhesive layer is prepared from the raw materials in Table 1 by weight:

[0066] Table 1 Raw materials of chloroprene rubber adhesive layer in Examples 1 to 4

[0067] raw material Mass Neoprene 100 Stearic acid 1 Magnesium oxide 3 Zinc Oxide 5 White Carbon Black 20 Adhesive RE 2 Accelerator H 1.5 Accelerator TMTD 1 Accelerator DM 1 sulfur 1.5

[0068] The surface adhesive layer is prepared from the raw materials in Table 2 by weight:

[0069] Table 2 Raw materials of the surface adhesive layer in Examples 1 to 4

[0070] raw materials Example 1 Example 2 Example 3 Example 4 Butyl rubber 100 / / / Chlorobutyl rubber / 100 / 50 Bromobutyl rubber / / 100 50 Diethyl azodicarboxylate 8 / 2 4 Benzenesulfonyl hydrazide / 6 / / p-Toluenesulfonyl hydrazide / / 4 3 Zinc stearate 2 4 4 3 White Carbon Black 20 18 10 16 Stearic acid 2 2 1 1 Zinc Oxide 5 5 2 3 sulfur 5 3 5 4 Protective wax 1.5 2 1.5 2 Antioxidant TMQ 2 1 3 3 Antioxidant 4426 3 5 3 2 Accelerator DM 0.3 0.8 0.5 1 Accelerator TMTD 1 0.5 0.8 0.5

[0071] The performance of the protective tapes prepared in Examples 1 to 4 was tested, and the test results are shown in Table 3:

[0072] Table 3 Performance test results of the protective tapes of Examples 1 to 4

[0073]

[0074]

[0075] It can be seen from Table 3 that the protective tape provided by the present invention has good structural strength, light weight, good air tightness, good heat resistance, cold resistance and acid and alkali resistance, can adhere well to fabrics, and has a stable structure.

[0076] It can be seen from the above embodiments that the protective tape provided by the present invention has the characteristics of good structural strength, high protective performance and light weight, and has excellent comprehensive performance, meeting the performance requirements for protective tape.

[0077] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A closed-cell rubber, It is characterized in that According to the weight percentage, it is prepared from the following raw materials: 100 parts of rubber, 5-8 parts of foaming agent, 2-4 parts of foaming aid, 10-20 parts of reinforcing filler, 1-2 parts of stearic acid, 2-5 parts of zinc oxide, 3-5 parts of sulfur, 1.5-2 parts of protective wax, 3-8 parts of antioxidant, and 0.8-2 parts of accelerator.

2. The closed-cell structure rubber according to claim 1, It is characterized in that The foaming agent is an organic foaming agent.

3. The closed-cell structure rubber according to claim 2, It is characterized in that The organic foaming agent includes one or more of azo compounds and sulfonyl hydrazide compounds.

4. The closed-cell rubber according to any one of claims 1 to 3, It is characterized in that The rubber includes one or more of butyl rubber, chlorinated butyl rubber and brominated butyl rubber.

5. A method for preparing the closed-cell structure rubber according to any one of claims 1 to 4, It is characterized in that The following steps are involved: The rubber, foaming agent, foaming aid, reinforcing filler, stearic acid, zinc oxide, sulfur, protective wax, antioxidant and accelerator are mixed and vulcanized to obtain closed-cell structure rubber.

6. The preparation method according to claim 5, It is characterized in that The vulcanization conditions are: heating from 100° C. to 140-145° C. and keeping the temperature, the heating time is 60 minutes, and the keeping time is 60-80 minutes.

7. A protective tape, It is characterized in that It includes an adhesive layer, a skeleton layer arranged on a side of the adhesive layer, and a surface adhesive layer arranged on the other side of the adhesive layer; The surface rubber layer is the closed-cell structure rubber described in any one of claims 1 to 4 or the closed-cell structure rubber obtained by the preparation method described in any one of claims 5 to 6.

8. The protective tape according to claim 7, It is characterized in that The thickness ratio of the surface rubber layer to the skeleton layer is 20-25:18-20; The thickness ratio of the surface glue layer to the adhesive layer is 20-25:1-2.

9. A method for preparing the protective tape according to any one of claims 7 to 8, It is characterized in that The following steps are involved: The surface of one side of the skeleton layer is coated with the raw material mixture of the adhesive layer, and then the surface adhesive layer is coated with the raw material mixture of the surface adhesive layer to obtain a multilayer body, and the multilayer body is vulcanized to obtain the protective tape.

10. Use of the protective tape according to any one of claims 7 to 8 or the protective tape obtained by the preparation method according to claim 9 in the fields of protective clothing, aerospace or transportation.