PVC (polyvinyl chloride) pipe and preparation method thereof

By combining modified styrene butadiene rubber and modified polyimide resin, combined with toughening agent and filler, the problem of insufficient toughness and impact resistance of PVC pipes is solved, the corrosion resistance and impact resistance are improved, and the corrosion resistance is reduced. The occurrence of production defects improves the overall performance of the material.

CN118931066APending Publication Date: 2024-11-12XINJIANG HONGNIAO WATER SAVING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411236578.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

PVC pipes have problems such as low toughness, poor impact resistance, unsuitable for hot water pipes, and prone to defects and chemical release during production.

Method used

Modified styrene butadiene rubber and modified polyimide resin are combined with toughening agents, fillers and lubricants to improve the corrosion resistance and toughness of the material through specific preparation methods, and are molded using a twin-screw extruder.

Benefits of technology

It improves the corrosion resistance, toughness and impact resistance of PVC pipes, reduces the occurrence of production defects, and enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027894850000121
    Figure BDA0005027894850000121
  • Figure BDA0005027894850000123
    Figure BDA0005027894850000123
  • Figure BDA0005027894850000131
    Figure BDA0005027894850000131
Patent Text Reader

Abstract

The invention discloses a PVC (polyvinyl chloride) pipe and a preparation method thereof. The PVC pipe is prepared from the following raw materials in parts by weight: 120-200 parts of polyvinyl chloride resin, 10-20 parts of modified styrene butadiene rubber, 10-20 parts of modified polyimide resin, 10-20 parts of a flexibilizer, 15-25 parts of filler, 1-3 parts of a lubricant, 1-3 parts of a plasticizer and 1-4 parts of a titanate coupling agent. The PVC pipe has the advantages of favorable corrosion resistance, favorable toughness and high mechanical strength. The combined use of the modified styrene butadiene rubber and the modified polyimide resin in the components improves the corrosion resistance of the material, the combined use of the chloroethyl acrylate-butadiene copolymer and the carboxyl-terminated nitrile rubber enhances the toughness of the material, and the basalt fiber and the green scale mineral powder are used as the composite filler to enhance the impact resistance of the material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of pipe manufacturing, and in particular relates to a PVC pipe and a preparation method thereof. Background Art

[0002] PVC pipe, or polyvinyl chloride pipe, is a plastic pipe widely used in various industrial and civil fields. PVC pipe has high tensile strength and impact resistance, and can withstand greater pressure and impact. PVC pipe has good corrosion resistance to corrosive media such as inorganic acids and alkalis, and is suitable for gas and liquid transportation in the chemical industry. Due to the smooth inner wall, the fluid resistance of PVC pipe is small, and a smaller pipe diameter can be used at the same flow rate, thus saving materials and costs. PVC pipe has good anti-aging performance and its normal service life can reach more than 50 years. The application of PVC pipe is very extensive, mainly including the following aspects: 1. Water supply and drainage system, PVC water supply pipes and drainage pipes are widely used in water supply and drainage systems of homes and public buildings. 2. Industrial application, PVC pipes are used for gas and liquid transportation, waste gas discharge, detoxification towers and other equipment in textile, chemical and other industries. 3. Municipal engineering, large-diameter PVC pipes are used for municipal sewage pipes, generally made into corrugated pipes, and can also be used as water pipes for field irrigation. 4. Electricity and communications: PVC power pipes have the characteristics of high strength, good flexibility, high temperature resistance, corrosion resistance, flame retardancy, and good insulation performance, and are suitable for the fields of electricity and communications.

[0003] PVC pipes are widely used in the fields of industry and construction, but they have some significant disadvantages, mainly including the following aspects: 1. Low toughness and poor impact resistance: PVC pipes have low toughness, which means they are brittle and have poor impact resistance. Therefore, before using PVC pipes and fittings, it is usually necessary to modify their toughness to improve their impact resistance. 2. Not suitable for hot water pipes: Although PVC pipes can be used as domestic water supply pipes, they are not suitable for direct drinking water supply pipes. This is because PVC pipes may release harmful substances such as chloride ions at high temperatures, which pose potential risks to human health. 3. Defects in the production process: PVC pipes are prone to various defects during the production process, such as moire, black lines, burnt lines, discoloration, etc. The direct cause of these defects is insufficient plasticization or insufficient material decomposition. In order to avoid these problems, it is necessary to strictly control the temperature of the extruder and the temperature of the head of each section. 4. Low flexibility: Compared with pipes made of other materials, PVC pipes have poor flexibility, are not easy to bend, and their main directions are straight. This makes PVC pipes more difficult to install and maintain. 5. Chemical Release: PVC pipes can produce hydrochloric acid fumes and release harmful chemicals in fire-related incidents, which pose a threat to the environment and human health. Summary of the invention

[0004] The object of the present invention is to provide a PVC pipe and a preparation method thereof.

[0005] A PVC pipe is made of the following raw materials in parts by weight: 120-200 parts of polyvinyl chloride resin, 10-20 parts of modified styrene-butadiene rubber, 10-20 parts of modified polyimide resin, 10-20 parts of toughening agent, 15-25 parts of filler, 1-3 parts of lubricant, 1-3 parts of plasticizer and 1-4 parts of titanate coupling agent.

[0006] Furthermore, the preparation method of the modified styrene butadiene rubber is as follows: 80-120 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 80-100 rpm, the plasticizing temperature is set to 80-90°C, and the plasticizing time of the raw rubber is set to 25-60s; the speed of the internal mixer is adjusted to 70-80 rpm, and then 0.3-0.8 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 90-120°C, and the mixing time is set to 2-4min to obtain the modified styrene butadiene rubber.

[0007] Furthermore, the preparation method of the modified polyimide resin is as follows: 40-60 parts of pyromellitic anhydride monomer are dissolved in 350-450 parts of dimethylacetamide according to weight parts, 40-50 parts of p-phenylenediamine monomer and 3-5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the reaction is carried out at 15-20° C. for 4-5 hours to obtain the modified polyimide resin.

[0008] Furthermore, the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1.

[0009] Furthermore, the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0010] Furthermore, the lubricant is one or more of microcrystalline wax, stearic acid, polypropylene wax, and polyethylene wax.

[0011] Furthermore, the plasticizer is one or more of di(2-ethylhexyl) phthalate, hydrogenated rosin, diisononyl phthalate, and diisodecyl phthalate.

[0012] Furthermore, the titanate coupling agent is one or more of tris(dioctylpyrophosphoryloxy)titanate isopropyl ester, tetraoctyloxytitanium [di(tridecyl phosphite)], and tetraoctyloxytitanium [di(dilauryl phosphite)].

[0013] The preparation method of the PVC pipe is carried out according to the following steps:

[0014] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110-130° C., and stopping stirring to obtain a premix;

[0015] (2) The premix is ​​conveyed to a cold mixer for stirring and cooling to 35-50°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding.

[0016] The processing temperature of the twin-screw extruder is 170-190°C.

[0017] Beneficial effects of the present invention: The PVC pipe of the present invention has good anti-corrosion performance, good toughness and high mechanical strength. The combination of modified styrene-butadiene rubber and modified polyimide resin in the components improves the anti-corrosion performance of the material, the combination of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber enhances the toughness of the material, and basalt fiber and green scale stone powder are used as composite fillers to enhance the impact resistance of the material. DETAILED DESCRIPTION

[0018] In order to facilitate the understanding of the present invention, the present invention will be described more fully below. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0019] Example 1

[0020] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 15 parts of modified styrene-butadiene rubber, 15 parts of modified polyimide resin, 15 parts of toughening agent, 20 parts of filler, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0021] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0022] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0023] The preparation method of the PVC pipe is carried out according to the following steps:

[0024] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0025] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0026] Example 2

[0027] A PVC pipe is made of the following raw materials in parts by weight: 130 parts of polyvinyl chloride resin, 12 parts of modified styrene-butadiene rubber, 12 parts of modified polyimide resin, 12 parts of toughening agent, 15 parts of filler, 1 part of stearic acid, 1 part of hydrogenated rosin, and 1 part of tetraoctyloxytitanium [di(tridecylphosphite)]; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0028] The preparation method of the modified styrene butadiene rubber is as follows: 80 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 80 rpm, the plasticizing temperature is set to 80° C., and the plasticizing time of the raw rubber is set to 30 s; the speed of the internal mixer is adjusted to 70 rpm, and then 0.4 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 90° C., and the mixing time is set to 2 min, to obtain the modified styrene butadiene rubber.

[0029] The preparation method of the modified polyimide resin is as follows: 40 parts of pyromellitic anhydride monomer are dissolved in 350 parts of dimethylacetamide according to weight parts, 40 parts of p-phenylenediamine monomer and 3 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the reaction is carried out at 15° C. for 4 hours to obtain the modified polyimide resin.

[0030] The preparation method of the PVC pipe is carried out according to the following steps:

[0031] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110° C., and then stopping stirring to obtain a premix;

[0032] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 35° C., then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 170° C.

[0033] Example 3

[0034] A PVC pipe is made of the following raw materials in parts by weight: 200 parts of polyvinyl chloride resin, 20 parts of modified styrene-butadiene rubber, 20 parts of modified polyimide resin, 20 parts of toughening agent, 25 parts of filler, 3 parts of polypropylene wax, 3 parts of diisodecyl phthalate, and 4 parts of tetraoctyloxytitanium [bis(dilauryl phosphite)]; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0035] The preparation method of the modified styrene butadiene rubber is as follows: 120 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 100 rpm, the plasticizing temperature is set to 90° C., and the plasticizing time of the raw rubber is set to 60 s; the speed of the internal mixer is adjusted to 80 rpm, and then 0.8 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 120° C., and the mixing time is set to 2 min, so as to obtain the modified styrene butadiene rubber.

[0036] The preparation method of the modified polyimide resin is as follows: 60 parts of pyromellitic anhydride monomer are dissolved in 450 parts of dimethylacetamide according to weight parts, 50 parts of p-phenylenediamine monomer and 5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the reaction is carried out at 20° C. for 5 hours to obtain the modified polyimide resin.

[0037] The preparation method of the PVC pipe is carried out according to the following steps:

[0038] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 130° C., and then stopping stirring to obtain a premix;

[0039] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 50° C., then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 190° C.

[0040] Comparative Example 1

[0041] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 30 parts of modified styrene-butadiene rubber, 15 parts of toughening agent, 20 parts of filler, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy) isopropyl titanate; the toughening agent is a mixture of ethyl chloride acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0042] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0043] The preparation method of the PVC pipe is carried out according to the following steps:

[0044] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0045] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0046] Comparative Example 2

[0047] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 30 parts of modified polyimide resin, 15 parts of toughening agent, 20 parts of filler, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0048] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0049] The preparation method of the PVC pipe is carried out according to the following steps:

[0050] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0051] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0052] Comparative Example 3

[0053] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 15 parts of modified styrene-butadiene rubber, 15 parts of modified polyimide resin, 15 parts of chloroethyl acrylate-butadiene copolymer, 20 parts of filler, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0054] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0055] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0056] The preparation method of the PVC pipe is carried out according to the following steps:

[0057] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0058] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0059] Comparative Example 4

[0060] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 15 parts of modified styrene-butadiene rubber, 15 parts of modified polyimide resin, 15 parts of carboxyl-terminated nitrile rubber, 20 parts of filler, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:1.

[0061] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0062] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0063] The preparation method of the PVC pipe is carried out according to the following steps:

[0064] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0065] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0066] Comparative Example 5

[0067] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 15 parts of modified styrene-butadiene rubber, 15 parts of modified polyimide resin, 15 parts of toughening agent, 20 parts of basalt fiber, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1.

[0068] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0069] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0070] The preparation method of the PVC pipe is carried out according to the following steps:

[0071] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0072] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0073] Comparative Example 6

[0074] A PVC pipe is made of the following raw materials in parts by weight: 180 parts of polyvinyl chloride resin, 15 parts of modified styrene-butadiene rubber, 15 parts of modified polyimide resin, 15 parts of toughening agent, 20 parts of green scale stone powder, 2 parts of microcrystalline wax, 2 parts of di(2-ethylhexyl) phthalate, and 3 parts of tri(dioctylpyrophosphoryloxy)titanate isopropyl; the toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:1.

[0075] The preparation method of the modified styrene butadiene rubber is as follows: 100 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 90 rpm, the plasticizing temperature is set to 85° C., and the plasticizing time of the raw rubber is set to 40 s; the speed of the internal mixer is adjusted to 75 rpm, and then 0.6 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 110° C., and the mixing time is set to 3 min, so as to obtain the modified styrene butadiene rubber.

[0076] The preparation method of the modified polyimide resin is as follows: 50 parts of pyromellitic anhydride monomer are dissolved in 400 parts of dimethylacetamide according to weight parts, 45 parts of p-phenylenediamine monomer and 4 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer are added, and the mixture is reacted at 18° C. for 4 hours to obtain the modified polyimide resin.

[0077] The preparation method of the PVC pipe is carried out according to the following steps:

[0078] (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 120° C., and then stopping stirring to obtain a premix;

[0079] (2) The premix is ​​conveyed to a cold mixer, stirred and cooled to 40°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding; the processing temperature of the twin-screw extruder is 180°C.

[0080] Experimental example:

[0081] Corrosion resistance, acid and alkali resistance: 10% hydrochloric acid, 40% sodium hydroxide and 50% sodium chloride were used to test the samples for corrosion. The results are shown in Table 1:

[0082] Table 1

[0083]

[0084] Tensile properties: tested with a universal testing machine in accordance with GB / T1040-92 and a test temperature of 25°C, with a tensile rate of 50 mm / min; Bending properties: tested with a universal testing machine in accordance with GB / T9341-2000 and a test temperature of 25°C, with a pressure head moving speed of 2 mm / min; each group of experiments was repeated 3 times to take the average value, and SPSS24.0 software was used for statistical analysis. The quantitative data results were used (mean ± standard deviation) was expressed, and the Kolmogorov-Smirnov test was used for data normality test. For data that met the normal distribution, the mean difference between the two groups was compared using the t test, and the difference was considered statistically significant when P < 0.05. The measurement results are shown in Table 2:

[0085] Table 2

[0086]

[0087]

[0088] Note: * represents P < 0.05 compared with the group in Example 1.

[0089] Impact performance: According to GB / T 1843-2008, the specimens were notched with a 2 mm gap for impact testing; each group of experiments was repeated 3 times to obtain the average value, and SPSS24.0 software was used for statistical analysis. The quantitative data results were used to (mean ± standard deviation), the Kolmogorov-Smirnov test was used for data normality test, and the t-test was used to compare the mean differences between the two groups for data that met the normal distribution, with P < 0.05 as the difference being statistically significant. The test results are shown in Table 3:

[0090] Table 3

[0091] Experimental Group <![CDATA[Impact strength kJ / m 2 > Example 1 5.62±0.23 Example 2 5.58±0.31 Example 3 5.65±0.27 Comparative Example 5 4.11±0.17* Comparative Example 6 4.08±0.24*

[0092] Note: * represents P < 0.05 compared with the group in Example 1.

[0093] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A PVC pipe, characterized in that: The invention is prepared from the following raw materials in parts by weight: 120-200 parts of polyvinyl chloride resin, 10-20 parts of modified styrene-butadiene rubber, 10-20 parts of modified polyimide resin, 10-20 parts of toughening agent, 15-25 parts of filler, 1-3 parts of lubricant, 1-3 parts of plasticizer and 1-4 parts of titanate coupling agent.

2. The PVC pipe according to claim 1, characterized in that: The preparation method of the modified styrene butadiene rubber is as follows: 80-120 parts of styrene butadiene rubber are added into an internal mixer according to weight proportions, the speed of the internal mixer is set to 80-100 rpm, the plasticizing temperature is set to 80-90° C., and the plasticizing time of the raw rubber is set to 25-60 s; the speed of the internal mixer is adjusted to 70-80 rpm, and then 0.3-0.8 parts of 4-mercaptobutyric acid are added into the internal mixer for mixing, the mixing temperature is set to 90-120° C., and the mixing time is set to 2-4 min to obtain the modified styrene butadiene rubber.

3. The PVC pipe according to claim 1, characterized in that: The preparation method of the modified polyimide resin comprises: dissolving 40-60 parts of pyromellitic anhydride monomer into 350-450 parts of dimethylacetamide according to weight parts, adding 40-50 parts of p-phenylenediamine monomer and 3-5 parts of 2,2-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane monomer, reacting at 15-20° C. for 4-5 hours, and obtaining the modified polyimide resin.

4. The PVC pipe according to claim 1, characterized in that: The toughening agent is a mixture of chloroethyl acrylate-butadiene copolymer and carboxyl-terminated nitrile rubber in a mass ratio of 2:

1.

5. The PVC pipe according to claim 1, characterized in that: The filler is a mixture of basalt fiber and green scale stone powder in a mass ratio of 1:

1.

6. The PVC pipe according to claim 1, characterized in that: The lubricant is one or more of microcrystalline wax, stearic acid, polypropylene wax and polyethylene wax.

7. The PVC pipe according to claim 1, characterized in that: The plasticizer is one or more of di(2-ethylhexyl)phthalate, hydrogenated rosin, diisononyl phthalate, and diisodecyl phthalate.

8. The PVC pipe according to claim 1, characterized in that: The titanate coupling agent is one or more of tris(dioctylpyrophosphoryloxy)titanate isopropyl ester, tetraoctyloxytitanium [di(tridecyl phosphite)], and tetraoctyloxytitanium [di(dilauryl phosphite)].

9. The method for preparing the PVC pipe according to claim 1, characterized in that: Follow these steps: (1) taking raw materials according to the formula, adding them into a high-speed mixer, stirring and heating to 110-130° C., and stopping stirring to obtain a premix; (2) The premix is ​​conveyed to a cold mixer for stirring and cooling to 35-50°C, and then discharged and conveyed to a twin-screw extruder for extrusion molding.

10. The method for preparing the PVC pipe according to claim 9, characterized in that: The processing temperature of the twin-screw extruder is 170-190°C.