Corrosion-resistant rubber plug assembly

Through the combination of modified fluoroelastomer and anti-permeable coating, the problem of poor corrosion resistance of rubber plugs is solved, which significantly improves corrosion resistance and service life, and ensures safety and stability in chemical liquid environments.

CN118931076APending Publication Date: 2024-11-12ANHUI ZHONGMA RUBBER & PLASTIC PROD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411245213.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing rubber plugs are prone to corrosion after contacting chemical liquid for a long time, which reduces service life and poses safety hazards, and has poor corrosion resistance.

Method used

Modified fluoro-rubber, ethylene-propylene rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant, plasticizer and anti-permeable coating are used to modify fluoro-rubber and in the rubber The plug surface is coated with a polytetrafluoroethylene coating to form a stable three-dimensional network structure and anti-permeability layer.

Benefits of technology

It significantly improves the corrosion resistance and service life of rubber plugs, enhances chemical stability and safety, effectively deals with various corrosive environments, extends service life and maintains stable performance.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a corrosion-resistant rubber plug assembly which is composed of the following components: 90-100 parts of modified fluororubber, 70-80 parts of ethylene propylene rubber, 15-20 parts of boron carbide, 20-25 parts of magnesium stearate, 15-20 parts of a vulcanization accelerator, 6-10 parts of a filler, 3-5 parts of a lubricant, 3-5 parts of a plasticizer and 3-5 parts of an anti-permeation coating. The modified fluororubber is used for replacing common fluororubber, so that the corrosion resistance of the fluororubber is remarkably improved, and the harsh industrial application requirements are met. According to the methods, the chemical stability of the material is enhanced, and the durability and safety of the material in actual use are also improved; the anti-permeation coating is coated on the surface of the rubber plug assembly, so that the diffusion rate of a chemical corrosive medium can be reduced, the rubber plug assembly can effectively cope with various corrosive environments, the service life of the rubber plug assembly is prolonged, and the performance stability of the rubber plug assembly is kept.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of medical rubber stoppers, in particular to a corrosion-resistant rubber stopper component. Background Art

[0002] Rubber stoppers are usually made of silicone rubber or fluororubber; rubber stoppers are very critical in laboratory and industrial applications. They are mainly used to seal containers to protect chemicals from the outside environment and to prevent environmental pollution or safety hazards caused by chemical leakage.

[0003] When in use, the rubber stopper needs to be in contact with chemical liquid for a long time, but the existing rubber stopper has poor corrosion resistance. After being in contact with chemical liquid for a long time, the rubber stopper is easily corroded and deteriorated, which not only reduces the service life of the rubber stopper but also poses a safety risk. Therefore, the present application proposes a rubber stopper assembly that can provide corrosion resistance to the rubber stopper. Summary of the invention

[0004] The object of the present invention is to provide a corrosion-resistant rubber plug assembly to solve the problems raised in the above background technology.

[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solution: a corrosion-resistant rubber plug assembly, composed of the following components: 90-100 parts of modified fluororubber, 70-80 parts of ethylene-propylene rubber, 15-20 parts of boron carbide, 20-25 parts of magnesium stearate, 15-20 parts of vulcanization accelerator, 6-10 parts of filler, 3-5 parts of lubricant, 3-5 parts of plasticizer, and 3-5 parts of anti-permeation coating.

[0006] According to an embodiment of the present invention, the modified fluororubber is prepared by modifying the fluororubber using a multifunctional cross-linking agent.

[0007] According to an embodiment of the present invention, the specific steps of modifying fluororubber with a multifunctional cross-linking agent are as follows:

[0008] The fluororubber is plasticized evenly on a double-roll mill and rolled to make the fluororubber reach appropriate plasticity for subsequent processing. During the entire plasticizing process, the roller temperature is controlled within 70-80℃;

[0009] Add the auxiliary materials and multifunctional aziridine crosslinking agent into the open mill, then cut left and right 3-6 times, then make triangle packs 5-10 times to ensure that the fluororubber, auxiliary materials and multifunctional aziridine crosslinking agent are fully mixed and evenly kneaded, and then adjust the roller distance to produce the sheet, and the thickness is controlled at 4-6mm;

[0010] The mixed rubber material is compressed into granules;

[0011] The formed granular rubber products are irradiated with high-energy rays generated by an electron accelerator;

[0012] During the irradiation process, the multifunctional aziridine crosslinking agent, under the action of radiation, triggers a crosslinking reaction between rubber molecular chains to form a stable three-dimensional network structure, thereby forming modified fluororubber.

[0013] According to an embodiment of the present invention, the mixing mass ratio of the fluororubber, auxiliary materials, and multifunctional aziridine cross-linking agent is 5:2:1.

[0014] According to an embodiment of the present invention, the auxiliary material consists of the following components: 5-8 parts of vulcanizing agent, 10-15 parts of carbon black, and 2-4 parts of sensitizer.

[0015] According to an embodiment of the present invention, the vulcanization accelerator is one of thiazoles and dithiophosphates.

[0016] According to an embodiment of the present invention, the filler is a mixture of white carbon black and calcium carbonate, and the weight ratio of the white carbon black to the calcium carbonate is 1:1.

[0017] According to an embodiment of the present invention, the lubricant is perfluoropolyether grease;

[0018] The plasticizer is a phthalate plasticizer.

[0019] According to an embodiment of the present invention, the anti-permeation coating is a polytetrafluoroethylene coating, which is formed by coating a layer of polytetrafluoroethylene solution on the surface of the molded rubber plug component.

[0020] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned corrosion-resistant rubber plug assembly, comprising the following steps:

[0021] Step 1: first prepare modified fluororubber;

[0022] Step 2, respectively weighing the modified fluororubber, ethylene-propylene rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant, and plasticizer according to weight;

[0023] Step 3, the modified fluororubber, EPDM rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant and plasticizer are mixed evenly, and the mixed raw materials are put into an internal mixer for mixing at a temperature of 105-115° C. for 10-15 minutes to obtain a mixed rubber and input it into a calender for calendering;

[0024] Step 4: Send the calendered rubber into a vulcanizer for vulcanization at a temperature of 125-135°C for 13-15 minutes. After vulcanization, the semi-finished product is edge-punched, cleaned and dried.

[0025] Step 5: Then, a layer of polytetrafluoroethylene solution is coated on the surface of the semi-finished product to form an anti-penetration coating, and then sterilization is performed to obtain a finished product.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] The present invention replaces ordinary fluororubber with modified fluororubber to significantly improve the corrosion resistance of fluororubber, thereby meeting more demanding industrial application requirements. These methods not only enhance the chemical stability of the material itself, but also improve its durability and safety in actual use;

[0028] By coating the surface of the rubber plug assembly with an anti-permeation coating, the diffusion rate of chemically corrosive media can be reduced, so that the rubber plug assembly can effectively cope with various corrosive environments, thereby extending its service life and maintaining its performance stability. DETAILED DESCRIPTION

[0029] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] According to a first aspect of the present invention, a corrosion-resistant rubber plug assembly is provided, consisting of the following components: 90-100 parts of modified fluororubber, 70-80 parts of ethylene-propylene rubber, 15-20 parts of boron carbide, 20-25 parts of magnesium stearate, 15-20 parts of vulcanization accelerator, 6-10 parts of filler, 3-5 parts of lubricant, 3-5 parts of plasticizer, and 3-5 parts of anti-permeation coating.

[0031] According to an embodiment of the present invention, the modified fluororubber is specifically modified by using a multifunctional cross-linking agent to modify the fluororubber, thereby significantly improving its corrosion resistance and comprehensive performance.

[0032] According to an embodiment of the present invention, the specific steps of modifying fluororubber with a multifunctional cross-linking agent are as follows:

[0033] The fluororubber is plasticized evenly on a double-roll mill and rolled to make the fluororubber reach appropriate plasticity for subsequent processing. During the entire plasticizing process, the roller temperature is controlled within 70-80℃ to avoid the adverse effects of high temperature on the performance of the fluororubber;

[0034] Add the auxiliary materials and multifunctional aziridine crosslinking agent into the open mill, then cut left and right 3-6 times, then make triangle packs 5-10 times to ensure that the fluororubber, auxiliary materials and multifunctional aziridine crosslinking agent are fully mixed and evenly kneaded, and then adjust the roller distance to produce the sheet, and the thickness is controlled at 4-6mm;

[0035] The mixed rubber material is compressed into granules;

[0036] The formed granular rubber products are irradiated with high-energy rays generated by an electron accelerator;

[0037] During the irradiation process, the multifunctional aziridine crosslinking agent, under the action of radiation, triggers a crosslinking reaction between rubber molecular chains to form a stable three-dimensional network structure, thereby forming modified fluororubber.

[0038] According to an embodiment of the present invention, the mixing mass ratio of fluororubber, auxiliary materials, and multifunctional aziridine cross-linking agent is 5:2:1.

[0039] According to an embodiment of the present invention, the auxiliary material consists of the following components: 5-8 parts of vulcanizing agent, 10-15 parts of carbon black, and 2-4 parts of sensitizer.

[0040] According to an embodiment of the present invention, the vulcanization accelerator is one of thiazoles and dithiophosphates.

[0041] According to an embodiment of the present invention, the filler is a mixture of white carbon black and calcium carbonate, and the weight ratio of white carbon black to calcium carbonate is 1:1.

[0042] According to an embodiment of the present invention, the lubricant is perfluoropolyether grease; and the plasticizer is a phthalate plasticizer.

[0043] According to an embodiment of the present invention, the anti-permeation coating is a polytetrafluoroethylene coating, which is formed by coating a layer of polytetrafluoroethylene solution on the surface of the molded rubber plug component.

[0044] According to a second aspect of the present invention, there is provided a method for preparing the above-mentioned corrosion-resistant rubber plug assembly, comprising the following steps:

[0045] Step 1: first prepare modified fluororubber;

[0046] Step 2, respectively weighing the modified fluororubber, ethylene-propylene rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant, and plasticizer according to weight;

[0047] Step 3, the modified fluororubber, EPDM rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant and plasticizer are mixed evenly, and the mixed raw materials are put into an internal mixer for mixing at a temperature of 105-115° C. for 10-15 minutes to obtain a mixed rubber and input it into a calender for calendering;

[0048] Step 4: Send the calendered rubber into a vulcanizer for vulcanization at a temperature of 125-135°C for 13-15 minutes. After vulcanization, the semi-finished product is edge-punched, cleaned and dried.

[0049] Step 5: Then, a layer of polytetrafluoroethylene solution is coated on the surface of the semi-finished product to form an anti-penetration coating, and then sterilization is performed to obtain a finished product.

[0050] The above-mentioned preparation scheme is adopted to prepare the rubber stopper assembly of the following embodiments, and the specific embodiments are shown as follows.

[0051] Example 1

[0052] A corrosion-resistant rubber plug assembly consists of the following components: 90 parts of modified fluororubber, 75 parts of ethylene-propylene rubber, 18 parts of boron carbide, 23 parts of magnesium stearate, 18 parts of dithiophosphate vulcanization accelerator, 5 parts of white carbon black, 5 parts of calcium carbonate, 4 parts of perfluoropolyether grease, 4 parts of phthalate plasticizer, and 4 parts of polytetrafluoroethylene coating.

[0053] Example 2

[0054] A corrosion-resistant rubber plug assembly consists of the following components: 100 parts of modified fluororubber, 75 parts of ethylene-propylene rubber, 18 parts of boron carbide, 23 parts of magnesium stearate, 18 parts of dithiophosphate vulcanization accelerator, 5 parts of white carbon black, 5 parts of calcium carbonate, 4 parts of perfluoropolyether grease, 4 parts of phthalate plasticizer, and 4 parts of polytetrafluoroethylene coating.

[0055] Comparative Example 1

[0056] A corrosion-resistant rubber plug assembly consists of the following components: 90 parts of fluororubber, 75 parts of ethylene-propylene rubber, 18 parts of boron carbide, 23 parts of magnesium stearate, 18 parts of dithiophosphate vulcanization accelerator, 5 parts of white carbon black, 5 parts of calcium carbonate, 4 parts of perfluoropolyether grease, 4 parts of phthalate plasticizer, and 4 parts of polytetrafluoroethylene coating.

[0057] The difference between this comparative example and Example 1 is that fluororubber is used instead of modified fluororubber, and the other components are the same, and the same preparation process is used.

[0058] Comparative Example 2

[0059] A corrosion-resistant rubber plug assembly consists of the following components: 90 parts of modified fluororubber, 75 parts of ethylene-propylene rubber, 18 parts of boron carbide, 23 parts of magnesium stearate, 18 parts of dithiophosphate vulcanization accelerator, 5 parts of white carbon black, 5 parts of calcium carbonate, 4 parts of perfluoropolyether grease, and 4 parts of phthalate plasticizer.

[0060] The difference between this comparative example and Example 1 is that the polytetrafluoroethylene coating is missing, the other components are the same, the preparation process of the rubber plug assembly is also the same, and after the rubber plug assembly is prepared, the polytetrafluoroethylene coating is not coated on the surface of the rubber plug assembly.

[0061] Comparative Example 3

[0062] A corrosion-resistant rubber plug assembly consists of the following components: 90 parts of fluororubber, 75 parts of ethylene-propylene rubber, 18 parts of boron carbide, 23 parts of magnesium stearate, 18 parts of dithiophosphate vulcanization accelerator, 5 parts of white carbon black, 5 parts of calcium carbonate, 4 parts of perfluoropolyether grease, and 4 parts of phthalate plasticizer.

[0063] The difference between this comparative example and Example 1 is that fluororubber is used instead of modified fluororubber, and the polytetrafluoroethylene coating is missing, and the other components are the same.

[0064] Experimental example

[0065] The rubber stopper assemblies prepared in Examples 1-2 of the present invention and the rubber stopper assemblies prepared in Comparative Examples 1-3 were subjected to performance tests, and the results are shown in Table 1 below:

[0066] Table 1 Performance test data

[0067] Group Example 1 Example 2 Comparative Example 1 Comparative Example 2 Comparative Example 3 Bending strength / MPa 96 104 56 63 42 Tensile strength / MPa 84 91 45 57 32 Alkali resistance / 60wt% NaOH solution 500h no change 500h no change There are cracks There are cracks There are cracks

[0068] It can be seen from the above table that the bending strength, tensile strength and alkali resistance (corrosion resistance) of the rubber plug assembly prepared in Examples 1-2 of the present application are better than those in Comparative Examples 1-3;

[0069] Specifically: By comparing the data of Example 1 and Comparative Example 1, it can be seen that when the modified fluororubber replaces the ordinary fluororubber, the bending strength, tensile strength and alkali resistance (corrosion resistance) of the rubber plug assembly are significantly improved, so the modified fluororubber can increase the strength and corrosion resistance of the rubber plug assembly;

[0070] By comparing the data of Example 1 and Comparative Example 2, it can be seen that by coating a layer of anti-permeation coating on the surface of the rubber plug assembly, the diffusion rate of the chemically corrosive medium can be reduced, so that the rubber plug assembly can effectively cope with various corrosive environments, thereby extending its service life and maintaining its performance stability;

[0071] By comparing the data of Example 1 and Comparative Example 3, it can be seen that by replacing ordinary fluororubber with a modified rubber plug and coating a layer of anti-permeation coating on the surface of the rubber plug assembly, the strength and corrosion resistance of the rubber plug assembly can be further improved.

[0072] The above-mentioned embodiments of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all the embodiments here. Any obvious changes or modifications derived from the technical solution of the present invention are still within the scope of protection of the present invention.

Claims

1. A corrosion-resistant rubber plug assembly, characterized in that: It is composed of the following components: 90-100 parts of modified fluororubber, 70-80 parts of ethylene-propylene rubber, 15-20 parts of boron carbide, 20-25 parts of magnesium stearate, 15-20 parts of vulcanization accelerator, 6-10 parts of filler, 3-5 parts of lubricant, 3-5 parts of plasticizer and 3-5 parts of anti-penetration coating.

2. A corrosion-resistant rubber plug assembly according to claim 1, characterized in that: The modified fluororubber is specifically prepared by modifying the fluororubber using a multifunctional crosslinking agent.

3. A corrosion-resistant rubber plug assembly according to claim 2, characterized in that: The specific steps of modifying fluororubber with a multifunctional crosslinking agent are as follows: The fluororubber is plasticized evenly on a double-roll mill and rolled to make the fluororubber reach appropriate plasticity for subsequent processing. During the entire plasticizing process, the roller temperature is controlled within 70-80℃; Add the auxiliary materials and multifunctional aziridine crosslinking agent into the open mill, then cut left and right 3-6 times, then make triangle packs 5-10 times to ensure that the fluororubber, auxiliary materials and multifunctional aziridine crosslinking agent are fully mixed and evenly kneaded, and then adjust the roller distance to produce the sheet, and the thickness is controlled at 4-6mm; The mixed rubber material is compressed into granules; The formed granular rubber products are irradiated with high-energy rays generated by an electron accelerator; During the irradiation process, the multifunctional aziridine crosslinking agent, under the action of radiation, triggers a crosslinking reaction between rubber molecular chains to form a stable three-dimensional network structure, thereby forming modified fluororubber.

4. A corrosion-resistant rubber plug assembly according to claim 3, characterized in that: The mixing mass ratio of the fluororubber, auxiliary materials and multifunctional aziridine cross-linking agent is 5:2:

1.

5. The corrosion-resistant rubber plug assembly according to claim 3, characterized in that: The auxiliary material consists of the following components: 5-8 parts of vulcanizing agent, 10-15 parts of carbon black and 2-4 parts of sensitizer.

6. The corrosion-resistant rubber plug assembly according to claim 1, characterized in that: The vulcanization accelerator is one of thiazoles and dithiophosphates.

7. The corrosion-resistant rubber plug assembly according to claim 1, characterized in that: The filler is a mixture of white carbon black and calcium carbonate, and the weight ratio of the white carbon black to the calcium carbonate is 1:

1.

8. The corrosion-resistant rubber plug assembly according to claim 1, characterized in that: The lubricant is perfluoropolyether grease; The plasticizer is a phthalate plasticizer.

9. The corrosion-resistant rubber plug assembly according to claim 1, characterized in that: The anti-permeation coating is a polytetrafluoroethylene coating, which is formed by coating a layer of polytetrafluoroethylene solution on the surface of the formed rubber plug component.

10. A method for preparing a corrosion-resistant rubber plug assembly according to any one of claims 1 to 9, characterized in that: The following steps are involved: Step 1: first prepare modified fluororubber; Step 2, respectively weighing the modified fluororubber, ethylene-propylene rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant, and plasticizer according to weight; Step 3, the modified fluororubber, EPDM rubber, boron carbide, magnesium stearate, vulcanization accelerator, filler, lubricant and plasticizer are mixed evenly, and the mixed raw materials are put into an internal mixer for mixing at a temperature of 105-115° C. for 10-15 minutes to obtain a mixed rubber and input it into a calender for calendering; Step 4: Send the calendered rubber into a vulcanizer for vulcanization at a temperature of 125-135°C for 13-15 minutes. After vulcanization, the semi-finished product is flushed, cleaned and dried. Step 5: Then, a layer of polytetrafluoroethylene solution is coated on the surface of the semi-finished product to form an anti-penetration coating, and then sterilization is performed to obtain a finished product.