Heat-resistant ABS composite material for vehicles and preparation method thereof

By adding thermoplastic polyurethane, modified fillers and silicone foamed microspheres to the ABS resin, combining chemical grafting treatment of amino acid nanotubes and montmorillonite, a porous frame structure is formed, and the ABS resin is solved. The problem of easy deformation in high-temperature environments improves its heat resistance and impact resistance.

CN118931100APending Publication Date: 2024-11-12QINGDAO MINGRUIXIANG PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411241276.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing ABS resins are prone to warping, deforming or softening in high temperature environments, and the addition of heat-resistant agents will affect their fluidity and impact resistance.

Method used

The combination materials such as thermoplastic polyurethane, modified fillers, silicone foamed microspheres and mixed fibers are used to improve the fluidity and interface performance of ABS resin through modification treatment, and enhance its heat resistance and impact resistance.

Benefits of technology

It improves the heat resistance and impact resistance of ABS composite materials, reduces internal stress in injection molding, and enhances molding stability and dimensional stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the field of high polymer materials, and particularly discloses a heat-resistant ABS composite material for a vehicle and a preparation method of the heat-resistant ABS composite material. The heat-resistant ABS composite material for the vehicle is prepared from the following raw materials in parts by weight: 80 to 90 parts of ABS resin, 10 to 20 parts of thermoplastic polyurethane, 10 to 20 parts of modified filler, 5 to 15 parts of organic silicon foaming microspheres, 0.1 to 1 part of lubricant, 0.1 to 1 part of antioxidant, 1 to 2 parts of flame retardant and 3 to 8 parts of mixed fiber. The ABS composite material provided by the invention has the advantages of strong heat resistance and good fluidity, is not easy to crack due to internal stress during injection molding, and has strong impact resistance, small molding shrinkage rate and good dimensional stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of polymer materials, and more specifically, to a heat-resistant automotive ABS composite material and a preparation method thereof. Background Art

[0002] As a plastic variety with excellent comprehensive physical and mechanical properties, ABS (styrene-acrylonitrile-butadiene copolymer) is increasingly widely used in the automotive, home appliances, machinery, textile and other industries. In recent years, with the continuous improvement of the lightweight level of automobiles, ABS is often used to manufacture automotive parts, such as dashboards, body panels, interior panels, steering wheels, sound insulation panels, door locks, bumpers, ventilation pipes, etc., and the demand for ABS resin in the automotive industry has increased rapidly. Most automotive parts are processed by injection molding. The advantages of ABS resin are better impact resistance, sound insulation, and scratch resistance. It is more beautiful than PP and is particularly suitable for parts with strict lateral impact resistance and use temperature.

[0003] In addition to having good physical and mechanical properties (especially impact resistance), ABS resin used in the manufacture of automotive parts must also have high heat resistance to meet the requirements of post-processing processes such as painting and more demanding use environments. Due to the structural and composition characteristics of ABS resin itself, the heat deformation temperature of ordinary ABS resin is lower than 85°C, and its long-term use temperature is only 80°C. When used in an environment above 90°C, it is often prone to the risk of warping, deformation, or even softening. ABS resin itself has good fluidity, but in order to improve its heat resistance, it is generally chosen to add heat-resistant agents, such as α-methylstyrene copolymer and N-phenylmaleimide copolymer. The addition of heat-resistant agents may change the molecular structure of ABS resin, increase the steric hindrance effect of the molecular chain, and affect the mobility of the molecules, thereby significantly reducing the fluidity of ABS resin. The reduction in fluidity will cause a large residual internal stress during the injection molding process, reduce the impact resistance of the injection molded product, and make the injection molded product prone to cracking. Summary of the invention

[0004] In order to improve the heat resistance and impact resistance of ABS materials and enhance their crack resistance, the present application provides a heat-resistant automotive ABS composite material and a preparation method thereof.

[0005] In the first aspect, the present application provides a heat-resistant automotive ABS composite material, which adopts the following technical solution: A heat-resistant ABS composite material for automobiles comprises the following raw materials in parts by weight: 80-90 parts of ABS resin, 10-20 parts of thermoplastic polyurethane, 10-20 parts of modified filler, 5-15 parts of organic silicon foam microspheres, 0.1-1 parts of lubricant, 0.1-1 parts of antioxidant, 1-2 parts of flame retardant and 3-8 parts of mixed fiber.

[0006] By adopting the above technical scheme, ABS resin is used as the base material, and a certain amount of thermoplastic polyurethane is added as a flow modifier. Since thermoplastic polyurethane is a linear block copolymer containing alternating hard segments and soft segments, it is widely used as a high-performance elastomer. Moreover, as the temperature changes, the intermolecular hydrogen bonds of thermoplastic polyurethane undergo cross-linking, so it has excellent tensile properties, low-temperature elasticity and wear resistance. The TPU-reinforced polymer has the characteristics of impact toughness and tear strength, excellent processing performance, etc., and has a toughening effect on ABS. TPU is an elastic polymer that can be processed and melted, and has a higher melt flow rate after melting. The fluidity of TPU in the molten state is much higher than that of ABS, and the polar groups in TPU can interact with the cyano groups in ABS. After TPU is added to ABS, the low-fluidity ABS will be driven by the high-fluidity TPU to flow together, so the flow performance of the composite material is improved. TPU is added to ABS for processing and molding. During the processing, since TPU has high fluidity in the molten state, it can make the mixture flow more easily in the cavity and runner, and the shearing effect on the melt will be reduced. During extrusion, the molecular chain orientation of the melt is small, which can reduce the residual stress of the product and make the material easier to process and mold. ABS itself has a certain toughness, and its toughening system is a rubber particle toughening system. Butadiene in ABS is a rubber particle, and rubber particles also exist in TPU. Rubber particles exist as stress concentration centers in composite materials. When the composite material is impacted, it can induce shear bands and silver streaks. The generation and development of these two requires energy absorption. At the same time, rubber particles can inhibit the unlimited growth of shear bands and silver streaks to prevent them from generating destructive cracks. Therefore, after adding TPU, the impact performance of the composite material is improved. Modified fillers can increase the interaction of hydrogen bonds within ABS and TPU. The enhancement of hydrogen bonds improves the ability of the composite material to resist deformation at high temperatures, thereby improving thermodynamic properties and Vicat softening temperature. Silicone foam microspheres have lower thermal expansion and contraction, low heat transfer coefficient and high strength. They play a role in hindering heat conduction and supporting during the injection molding cooling process, thereby enhancing the ability of the composite material to resist cooling shrinkage deformation, thereby enhancing the ability of injection molded products to resist deformation and cracking. In addition, silicone foam microspheres have a three-dimensional porous structure and a mesh structure, which can effectively inhibit molecular motion and improve the thermal stability of the material, thereby improving heat resistance.

[0007] Optionally, the silicone foamed microspheres are pretreated as follows: The organic silicon foam microspheres are immersed in a concentrated nitric acid solution, reacted at 80-85° C. for 1-2 hours, and vacuum dried to obtain carboxylated organic silicon foam microspheres; In parts by weight, 25-30 parts of halloysite nanotubes and 25-30 parts of montmorillonite are subjected to amination modification to obtain an amination mixture, the amination mixture is added to 200-250 parts of DMF solution, ultrasonicated to obtain a suspension, and 400-500 parts of Carboxylated silicone foam microspheres and 40-50 parts of phosphate ester are stirred at room temperature for 20-24 hours, filtered, and vacuum dried.

[0008] By adopting the above technical scheme, the surface of the silicone foam microsphere is smooth and inert, which makes its interface bonding with materials such as ABS resin not ideal. Therefore, the silicone foam microsphere is treated with a mixture, using one-dimensional tubular halloysite nanotubes and two-dimensional flaky montmorillonite, both of which have excellent mechanical properties, and inorganic materials of different dimensions have anisotropy in the load transfer direction, which can effectively enhance the interface performance of the silicone foam microsphere and the ABS resin. In addition, the halloysite nanotubes and montmorillonite are grafted on the silicone foam microspheres by chemical grafting, so that the silicone foam microspheres and the ABS resin have good bonding strength. The amino-treated halloysite nanotubes and montmorillonite are used. The organic silicon foam microspheres are rich in terminal reactive groups, and the organic silicon foam microspheres oxidized with concentrated nitric acid are rich in carboxyl groups. Halloysite nanotubes and montmorillonite are grafted onto the organic silicon foam microspheres through amide reaction, and reactive active functional groups are introduced into the organic silicon foam microspheres in the form of chemical bonds. The active functional groups will increase the chemical interaction, mechanical interlocking and wettability with ABS resin, and further improve the interface properties of organic silicon foam microsphere reinforced composite materials, thereby improving the impact resistance and mechanical strength of ABS composite materials. In addition, the thermal conductivity coefficients of halloysite nanotubes and montmorillonite are small, which can hinder heat conduction, reduce cooling shrinkage deformation and improve molding stability when the ABS composite materials are injection molded.

[0009] Optionally, the amino modification of the halloysite nanotubes and montmorillonite is modification with a silane coupling agent.

[0010] By adopting the above technical scheme, the silane coupling agent can form a durable bond between organic and inorganic materials, functionalize the surface of halloysite nanotubes and montmorillonite, and contain amino groups on the surface, which is convenient for the amidation reaction with the carboxyl groups on the carboxylated organic foaming microspheres.

[0011] Optionally, the mixed fiber includes basalt fiber and polyetheretherketone fiber in a mass ratio of 0.1-0.3:1.

[0012] By adopting the above technical solution, basalt fiber exhibits a very wide operating temperature range and excellent high temperature resistance, and can nucleate at very high temperatures. Polyetheretherketone fiber is a high-performance polymer fiber with excellent heat resistance and a melting point of more than 300°C, which enables it to maintain its structure and performance stability in high temperature environments. It also has good chemical stability and mechanical strength. Therefore, the combination of the two fibers can improve the heat resistance, rigidity and strength of ABS composite materials, and make the composite materials less likely to deform during injection molding.

[0013] Optionally, the mixed fiber is pretreated as follows: The mixed fiber is treated with a sodium dodecylbenzene sulfonate solution with a concentration of 4-5wt%, and then dispersed in deionized water after drying, and silica sol and agarose are added, and the temperature is raised to 85-90°C, mixed evenly, and then freeze-dried, and then heated to 380-400°C, and kept warm for 2-2.5h to form a fiber skeleton, and the mass ratio of the mixed fiber, silica sol and agarose is 1:6-8:0.25-0.3; The fiber skeleton is added into a 4-5wt% hexadecyltrimethylammonium chloride solution for immersion modification, washed, dried, and crushed to 3-6 mm.

[0014] By adopting the above technical scheme, sodium dodecylbenzene sulfonate is first used to remove impurities on the surface of the mixed fiber, and then silica sol and agarose are used as binders to overlap the mixed fibers. Silica sol, as a high-temperature inorganic binder, plays a role in bonding the fibers to build the overall framework of the skeleton. Agarose is a low-temperature organic binder, which can not only play a role in bonding short-cut fibers at low temperatures, but also play a role in pore formation when decomposed at high temperatures. During high-temperature treatment, the agarose inside the skeleton is decomposed into water and carbon dioxide at high temperatures, and the fibers in the fiber skeleton are overlapped into a bird's nest-like structure. The molten silica sol at 380-400°C flows to the fiber overlap point to play a secondary bonding role. After the heat treatment is completed, the hot-melt silica sol solidifies and the fibers are bonded. , forming a porous framework structure; then, the porous framework structure is hydrophobically modified by using hexadecyltrimethylammonium chloride. There are a large number of hydrophilic hydroxyl groups on the porous skeleton. These hydroxyl groups will undergo obvious volume shrinkage after dehydration condensation, thereby destroying the skeleton structure. The skeleton is hydrophobically treated so that the hydrophilic hydroxyl groups are replaced by hydrophobic methyl groups, which is convenient for increasing the dispersibility and compatibility of the mixed fiber in matrices such as ABS. When the ABS composite is heated, the porous framework structure formed by the mixed fiber can limit the movement of the polymer chain when heated, so that the movement of the molecular chain is restricted, reducing the deformation or damage of the material caused by thermal movement, enhancing the heat resistance of the composite material, and increasing the impact resistance and deformation resistance of the material.

[0015] Optionally, the modified filler includes hollow glass microspheres with a particle size of 10-45 μm, acrylic artificial stone waste powder with a particle size of 100-125 μm, and nano-silicon dioxide with a diameter of ≤50 nm in a mass ratio of 0.3-0.6:0.1-0.3:1.

[0016] By adopting the above technical scheme, the hollow glass microbeads are in the shape of tiny spheres, which have good fluidity in liquid resin. The spherical hollow glass microbeads are easier to disperse evenly in the resin, and their oil absorption value is low, which has little effect on the viscosity of the system, thereby helping to improve the fluidity of ABS resin; acrylic artificial stone is obtained by polymerizing methyl methacrylate, ultrafine aluminum hydroxide, natural pigments and the like as raw materials. The product is non-toxic, non-radioactive, oil-free, non-fouling, antibacterial and mildew-proof, impact-resistant, and anti-aging, and is widely used. However, acrylic artificial stone needs to be cut, ground, polished and other processes during production, which will produce a large amount of waste containing aluminum hydroxide, which can improve the thermal stability of the composite material and increase the Vicat softening point. Nano-silicon dioxide in the polymer matrix can not only toughen the matrix by effectively transferring the load, but also reinforce the matrix to improve the impact resistance and thermal properties.

[0017] Optionally, the modified filler is prepared as follows: adding polyethersulfone to dichloromethane, stirring and dissolving, and preparing a modified liquid with a concentration of 8-10wt%; Hollow glass microspheres, acrylic artificial stone waste powder and nano-silicon dioxide are mixed to prepare mixed powder, which is added to the modified liquid, stirred for 2-4 hours, dried at 210-230°C for 3-4 hours, and crushed. The amount of the mixed powder added is 4-5wt% of the amount of the modified liquid.

[0018] By adopting the above technical scheme, polyethersulfone is a special thermoplastic polymer material with high toughness, heat resistance and small thermal expansion coefficient. There are sulfone groups with excellent heat resistance on the molecular chain. When polyethersulfone is introduced into the surface of the filler, the heat resistance of the blending system is increased. Polyethersulfone is distributed on three fillers and dispersed in the ABS matrix in the form of particles to form an island structure. The spherical particles of polyethersulfone serve as a stress concentration source when the ABS resin breaks, preventing the expansion of cracks and changing the development direction of cracks, inhibiting them from developing into destructive cracks, and absorbing energy. In addition, when mixed materials such as ABS are damaged by external forces, polyethersulfone undergoes plastic deformation, effectively inhibiting crack expansion, absorbing part of the energy, improving the impact resistance of the composite material, hindering the generation of cracks, and improving the toughness of the composite material. In addition, the heat conduction of the modified filler is reduced, heat conduction is hindered during injection cooling, cooling shrinkage deformation is resisted, and molding stability is increased.

[0019] Optionally, the melt index of the ABS is 40-50 g / 10 min.

[0020] By adopting the above technical solution and using ABS resin with a higher melt index as the base material, the fluidity of the composite material can be improved, the flow resistance during the injection molding process can be reduced, the internal stress can be reduced, and the plastic molecules can be prevented from being oriented during the process of filling the mold during injection molding, and cracking due to large internal stress generated during cooling.

[0021] Optionally, the antioxidant is one or more of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 2-hydroxy-4-n-octyloxybenzophenone; The flame retardant is one or more of triphenyl phosphate, melamine cyanurate, and inorganic filler; The lubricant is one or more of silicone oil, white mineral oil, fatty acid amide, stearate, paraffin, polyethylene wax or ethylene bisstearamide.

[0022] By adopting the above technical scheme, the flame retardant in the ABS composite material can make the ABS composite material have better flame retardancy, so that it is not easy to burn or slow down the burning speed when encountering a fire source, thereby reducing the risk of fire; the antioxidant can prevent the composite material from being degraded due to oxidation during processing, storage and use, thereby extending the service life of the product, maintaining its physical properties and appearance, inhibiting harmful substances produced by oxidation, and improving the safety and environmental protection of the product; the lubricant can reduce adhesion or abrasion of the composite material during processing, improve the smoothness of the product surface, and help the uniform mixing and flow of the material.

[0023] In a second aspect, the present application provides a method for preparing a heat-resistant automotive ABS composite material, which adopts the following technical solution: A method for preparing a heat-resistant ABS composite material for automobiles comprises the following steps: Dry the ABS resin and thermoplastic polyurethane at 80-90°C for 6-8h, mix them evenly, extrude and granulate them to make mixed masterbatch; The mixed masterbatch, modified filler, organic silicon foam microsphere, lubricant, antioxidant, flame retardant and mixed fiber are uniformly mixed, extruded and granulated to obtain a composite material.

[0024] By adopting the above technical solution, ABS resin and thermoplastic polyurethane are first mixed and granulated, so that there is a good interface bonding force between the two, and the impact performance of the composite material is increased.

[0025] In summary, this application has the following beneficial effects: 1. Since the present application uses thermoplastic polyurethane, silicone foam microspheres, modified fillers and mixed fibers to treat ABS resin, thermoplastic polyurethane can increase the fluidity of ABS resin and reduce injection molding internal stress, silicone foam microspheres can hinder the movement of polymer chains under heat and increase heat resistance, and modified fillers and mixed fibers can further improve heat resistance and molding stability during injection molding.

[0026] 2. In the present application, it is preferred to mix amination of halloysite nanotubes and amination of montmorillonite with carboxylated silicone foam microspheres to allow the three to undergo an amidation reaction, graft halloysite nanotubes and montmorillonite onto the silicone foam microspheres through chemical grafting, and use hexadecyltrimethylammonium chloride to perform hydrophobic modification on them, thereby increasing the dispersibility and compatibility of the silicone foam microspheres in the resin material and improving mechanical strength such as impact resistance.

[0027] 3. In the present application, silica sol and agarose are preferably used as binders to mix polyetheretherketone fiber and basalt fiber, and a porous framework structure is obtained by heat treatment and freeze drying, thereby hindering the movement of molecular chains and improving the heat resistance of the composite material. DETAILED DESCRIPTION

[0028] The following examples further illustrate the present application in detail.

[0029] Preparation example of modified filler Preparation Example 1: 38 g of polyethersulfone was added to dichloromethane, stirred and dissolved to obtain a modified liquid with a concentration of 10 wt%. The polyethersulfone was selected from BASF of Germany, and the model was E6020P; 6g of hollow glass microspheres, 3g of acrylic artificial stone waste powder and 10g of nano-silicon dioxide are mixed to prepare a mixed powder, which is added to the modified liquid, stirred for 4 hours, and dried at 210°C for 4 hours. The amount of mixed powder added is 5wt% of the amount of the modified liquid. The particle size of the hollow glass microspheres is 10-45μm, selected from Guangdong Zhaotong Glass Plastic, model 3010, the particle size of the acrylic artificial stone waste powder is 125μm, and the particle size of the nano-silicon dioxide is 50nm.

[0030] Preparation Example 2: 28 g of polyethersulfone was added to dichloromethane, stirred and dissolved to obtain a modified liquid with a concentration of 10 wt%, wherein the polyethersulfone was selected from BASF of Germany, and the model number was E6020P; 3g of hollow glass microspheres, 1g of acrylic artificial stone waste powder and 10g of nano-silicon dioxide are mixed to prepare a mixed powder, which is added to the modified liquid, stirred for 4 hours, and dried at 210°C for 4 hours. The amount of mixed powder added is 4wt% of the amount of the modified liquid. The particle size of the hollow glass microspheres is 10-45μm, selected from Guangdong Zhaotong Glass Plastic, model 3010, the particle size of the acrylic artificial stone waste powder is 100μm, and the particle size of the nano-silicon dioxide is 50nm.

[0031] Preparation Example 3: The difference from Preparation Example 1 is that the particle sizes of the hollow glass microspheres, acrylic artificial stone waste powder and silicon dioxide are all 125 μm.

[0032] Preparation Example 4: The difference from Preparation Example 1 is that equal amounts of hollow glass microspheres are used to replace acrylic artificial stone waste powder and nano-silicon dioxide. Example

[0033] Example 1: A heat-resistant ABS composite material for automobiles, the raw material dosage is shown in Table 1, wherein the melt index of the ABS resin is 50g / 10min, and the density is 1.04g / cm 3 , selected from Taiwan Formosa Chemical Corporation, model AF3535, thermoplastic polyurethane density is 1.24g / cm 3 , selected from BASF, Germany, model S95A, the modified filler is made by Preparation Example 1, the silicone foam microsphere is a porous silicone rubber, selected from Shanghai Hengfei Biotechnology Co., Ltd., China, model DG-3, particle size 80-100 mesh, lubricant is silicone oil, antioxidant is tetrakis (β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate) pentaerythritol ester, flame retardant is triphenyl phosphate, mixed fiber includes basalt fiber and polyetheretherketone fiber with a mass ratio of 0.3:1, and the length of basalt fiber and polyetheretherketone fiber is 6mm; The method for preparing the heat-resistant automotive ABS composite material comprises the following steps: ABS resin and thermoplastic polyurethane are dried at 80°C for 8h, mixed evenly, extruded and granulated to make mixed masterbatch. The temperatures from barrel to die during extrusion are 170°C, 185°C, 190°C, 195°C, 200°C, 200°C and 205°C respectively. The mixed masterbatch, modified filler, silicone foam microspheres, lubricant, antioxidant, flame retardant and mixed fiber are mixed evenly, extruded and granulated to make composite materials. The temperatures are 210, 220, 225, 225 and 215°C respectively, and the nozzle is 215°C.

[0034] Table 1 Amount of raw materials used for ABS composite materials in Examples 1-3 Example 2: A heat-resistant ABS composite material for automobiles, the raw material dosage is shown in Table 1, wherein the melt index of the ABS resin is 40g / 10min, and the density is 1.04g / cm 3 , selected from Taiwan Formosa Chemical Corporation, model AF3500, thermoplastic polyurethane density is 1.24g / cm 3, selected from BASF of Germany, model S95A, the modified filler is made by Preparation Example 2, the silicone foam microsphere is porous silicone rubber, selected from Shanghai Hengfei Biotechnology Co., Ltd. of China, model DG-3, particle size is 80-100 mesh, lubricant is paraffin, antioxidant is 2-hydroxy-4-n-octyloxybenzophenone, flame retardant is melamine cyanurate, mixed fiber includes basalt fiber and polyetheretherketone fiber with a mass ratio of 0.3:1, and the length of basalt fiber and polyetheretherketone fiber is 3mm; The method for preparing the heat-resistant automotive ABS composite material comprises the following steps: ABS resin and thermoplastic polyurethane are dried at 90°C for 6 hours, mixed evenly, extruded and granulated to make mixed masterbatch. The temperatures from barrel to die during extrusion are 170°C, 185°C, 190°C, 195°C, 200°C, 200°C and 205°C respectively. The mixed masterbatch, modified filler, silicone foam microspheres, lubricant, antioxidant, flame retardant and mixed fiber are mixed evenly, extruded and granulated to make a composite material. The temperatures are 210, 220, 225, 225 and 215°C respectively, and the nozzle is 215°C.

[0035] Example 3: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the amounts of raw materials used are as shown in Table 1.

[0036] Example 4: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the modified filler is made from Preparation Example 3.

[0037] Example 5: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the modified filler is made from Preparation Example 4.

[0038] Example 6: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the mixed fibers are all polyetheretherketone fibers.

[0039] Example 7: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the mixed fiber is pretreated as follows: The basalt fiber and the polyetheretherketone fiber are mixed evenly to obtain a mixed fiber, and then 50g of the mixed fiber is immersed in a 5wt% sodium dodecylbenzene sulfonate solution for 30min, dried at 60°C and dispersed in 1000g deionized water, and silica sol and agarose are added, heated to 90°C, mixed evenly, freeze-dried at -60°C for 24h, and then heated to 380°C and kept warm for 2.5h to form a fiber skeleton, the mass ratio of the mixed fiber, silica sol and agarose is 1:8:0.3, and the silica sol is selected from Guangdong Huihe Silicon Products, model S-515; The fiber skeleton was added to a 5 wt % hexadecyltrimethylammonium chloride solution and immersed for 40 min, washed with deionized water, vacuum dried at 80° C. for 24 h, and crushed to 6 mm.

[0040] Embodiment 8: A heat-resistant ABS composite material for automobiles, which is different from Embodiment 1 in that the mixed fiber is pretreated as follows: The basalt fiber and the polyetheretherketone fiber are mixed evenly to obtain a mixed fiber, and then 50g of the mixed fiber is immersed in a 4wt% sodium dodecylbenzene sulfonate solution for 30min, dried at 60°C and dispersed in 1000g deionized water, and silica sol and agarose are added, heated to 85°C, mixed evenly, freeze-dried at -60°C for 24h, and then heated to 400°C and kept warm for 2h to form a fiber skeleton, the mass ratio of the mixed fiber, silica sol and agarose is 1:6:0.25, and the silica sol is selected from Guangdong Huihe Silicon Products, model S-515; The fiber skeleton was added to a 4 wt % hexadecyltrimethylammonium chloride solution and immersed for 40 min, washed with deionized water, vacuum dried at 80° C. for 24 h, and crushed to 3 mm.

[0041] Example 9: A heat-resistant ABS composite material for automobiles, which differs from Example 7 in that the fiber skeleton is not impregnated with a hexadecyltrimethylammonium chloride solution.

[0042] Example 10: A heat-resistant ABS composite material for automobiles, which differs from Example 7 in that silica sol and agarose are not added.

[0043] Example 11: A heat-resistant ABS composite material for automobiles, which is different from Example 7 in that the organic silicone foamed microspheres are pretreated as follows: The organic silicon foam microspheres were immersed in a concentrated nitric acid solution, the mass ratio of the organic silicon foam microspheres to the concentrated nitric acid solution was 1:30, reacted at 80°C for 2h, filtered, and vacuum dried at 60°C for 24h to obtain carboxylated organic silicon foam microspheres; 30 g of halloysite nanotubes and 30 g of montmorillonite were mixed to prepare a mixture, which was dispersed into 150 g of a mixed solution of ethanol and deionized water in a mass ratio of 1:4, 2 g of a silane coupling agent KH550 was added, and the mixture was stirred at room temperature for 24 h, vacuum filtered, washed, and vacuum dried at 50° C. to obtain an amino mixture, wherein the particle size of the halloysite nanotubes was 800 mesh, and the particle size of the montmorillonite was 1000 mesh; The amination mixture was added to 250 g of DMF solution, ultrasonicated for 20 min to obtain a suspension, 500 g of carboxylated silicone foam microspheres and 50 g of phosphate ester were added, stirred at room temperature for 24 h, filtered and then vacuum dried at 80° C. for 24 h.

[0044] Example 12: A heat-resistant ABS composite material for automobiles, which is different from Example 7 in that the organic silicone foamed microspheres are pretreated as follows: The organic silicon foam microspheres were immersed in a concentrated nitric acid solution, the mass ratio of the organic silicon foam microspheres to the concentrated nitric acid solution was 1:30, reacted at 85°C for 1 hour, filtered, and vacuum dried at 60°C for 24 hours to obtain carboxylated organic silicon foam microspheres; 25 g of halloysite nanotubes and 25 g of montmorillonite were mixed to prepare a mixture, which was dispersed into 130 g of a mixed solution of ethanol and deionized water in a mass ratio of 1:4, 2 g of a silane coupling agent KH550 was added, and the mixture was stirred at room temperature for 24 h, vacuum filtered, washed, and vacuum dried at 50° C. to obtain an amino mixture, wherein the particle size of the halloysite nanotubes was 800 mesh, and the particle size of the montmorillonite was 1000 mesh; The amination mixture was added to 200 g of DMF solution and ultrasonicated for 20 min to obtain a suspension, 400 g of carboxylated silicone foam microspheres and 40 g of phosphate were added, stirred at room temperature for 20 h, filtered and then vacuum dried at 80° C. for 24 h.

[0045] Example 13: A heat-resistant automotive ABS composite material, which differs from Example 11 in that an equal amount of carbon nanotubes is used to replace halloysite nanotubes and montmorillonite, and the carbon nanotubes are DZ-300, with a length of 5-20 μm, a fineness of 8-15 nm, and a density of 2.1 g / cm 3 .

[0046] Example 14: A heat-resistant ABS composite material for automobiles, which is different from Example 11 in that the halloysite nanotubes and montmorillonite are not subjected to amination treatment.

[0047] Comparative Example Comparative Example 1: A heat-resistant ABS composite material for automobiles, which is different from Example 1 in that the filler is not modified.

[0048] Comparative Example 2: A heat-resistant ABS composite material for automobiles, which differs from Example 1 in that no mixed fiber is added.

[0049] Comparative Example 3: A heat-resistant ABS composite material for automobiles, which differs from Example 1 in that silicone foamed microspheres are not added.

[0050] Comparative Example 4: A heat-resistant ABS composite material for automobiles, which differs from Example 1 in that an equal amount of ABS resin is used to replace thermoplastic polyurethane, and the melt index of the ABS resin is 50 g / 10 min and the density is 1.04 g / cm 3 , selected from Formosa Chemical Corporation of Taiwan, China, model number is AF3535.

[0051] Comparative Example 5: A high heat-resistant antistatic ABS material, including 63.5kg ABS, 15kg PA6, 18kg antistatic agent, 3kg compatibility modifier and 0.5kg antioxidant, ABS is AG12A1 of Formosa Chemical, A6 is PA6CSR / OS of Xinhui Meida, the antistatic agent is polyamide-polyether block copolymer, PebaxMV1074 of Arkema; ​​the compatibility modifier is styrene-N-phenyl maleimide-maleic anhydride copolymer, MS-L2A of Nippon Electric Chemical; the antioxidant is β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, BASF 1076. The preparation method, the steps are as follows: (1) ABS, PA6, antistatic agent, compatibility modifier and other additives are placed in a high-speed mixer and mixed for 3 minutes before discharging to obtain a mixture; (2) the mixture is placed in a twin-screw extruder for extrusion and granulation to obtain a high heat-resistant antistatic ABS material; the processing temperature of the twin-screw extruder is 220° C., and the screw speed is 400 rpm.

[0052] Performance testing The ABS composite material was prepared according to the methods in the examples and comparative examples, and the performance was tested according to the following methods. The test results are recorded in Table 2.

[0053] 1. Impact strength: The composite material was injection molded into a specimen, and five temperature sections were set at 230, 235, 240, 245, and 250°C, the injection pressure was 120MPa, the screw speed was 40rad / min, the injection time was 5s, and the holding time was 10s. The specimen was tested in accordance with GB / T1043-2008 "Determination of impact properties of simply supported beams of plastics".

[0054] 2. Tensile strength: The composite material was injection molded into a specimen, and five temperature sections were set at 230, 235, 240, 245, and 250°C, the injection pressure was 120 MPa, the screw speed was 40 rad / min, the injection time was 5 s, and the holding time was 10 s. The specimen was tested in accordance with GB / T1040-2006 "Determination of rate tensile properties Part 1: General principles".

[0055] 3. Melt flow rate: After drying the pellets of the composite material, take out an appropriate amount of the composite material and place it in the MFI450D melt index instrument. The test temperature is set to 220°C, the load is 10kg, ten samples are cut, and the cutting time is 5s; after the test, the average ratio of each sample is weighed with an electronic scale, and the data is input into the instrument to obtain the melt index of the composite material. The samples of each embodiment are tested three times to obtain the average value, thereby reducing the error of the test and improving the reliability of the data.

[0056] 4. Vicat softening temperature: According to GB / T1633-2000 "Determination of the Vicat softening temperature (VST) of thermoplastic materials", the heating rate is 50℃ / h and the load is 1kg.

[0057] 5. Molding shrinkage: Tested in accordance with ASTM D955-2008 "Standard Test Method for Measurement of Model Dimensional Shrinkage of Thermoplastics"; Table 2 Performance test of ABS composite materials Combining Examples 1-3 and the data in Table 2, it can be seen that the modified fillers prepared in Preparation Examples 1 and 2, using ABS resin with a higher melt index, and using polyetheretherketone fiber and basalt fiber as composite fibers can effectively improve the melt index of ABS, improve fluidity, increase impact strength and tensile strength, increase crack resistance, reduce molding shrinkage, and increase dimensional stability.

[0058] Compared with Example 1, Examples 4 and 5 respectively use the modified fillers prepared in Preparation Examples 3 and 4. Table 2 shows that the impact strength and tensile strength of the ABS composite material prepared in Example 4 decrease, the melt flow rate decreases, the molding shrinkage rate of the composite material prepared in Example 5 increases, the heat transfer effect is higher than that in Example 1, and the thermal expansion and contraction phenomenon is more obvious.

[0059] Compared with Example 1, Example 6 only uses polyetheretherketone fiber. Table 2 shows that the impact resistance and tensile strength of the composite material prepared in Example 6 are reduced, the melt flow rate and molding shrinkage rate do not change much, and the Vicat softening temperature decreases slightly.

[0060] In Examples 7 and 8, the mixed fibers were pretreated with silica sol and agarose to form a porous framework structure. The data in Table 2 show that the impact strength and tensile resistance of the ABS composite material are improved, but its melt flow rate is affected to a certain extent. However, its Vicat softening temperature is increased, the shrinkage rate is reduced, and the heat resistance and dimensional stability are improved.

[0061] In Example 9, compared with Example 7, the fiber skeleton is not subjected to hydrophobic treatment with the hexadecyltrimethylammonium chloride solution, and the dispersibility of the fiber skeleton in the resin matrix is ​​affected, resulting in a decrease in the impact strength and other properties of the composite material.

[0062] In Example 10, compared with Example 7, no silica sol and agarose were added. As shown in Table 2, the impact resistance and tensile strength of the composite material decreased, the Vicat softening temperature decreased, and the molding shrinkage increased, indicating that the use of silica sol and agarose can form a porous skeleton structure and improve the mechanical properties, heat resistance and dimensional stability of the composite material.

[0063] Compared with Example 7, Example 11 and Example 12 also pre-treated the silicone foamed microspheres, and the impact strength and tensile strength of the composite materials were increased, the melt flow rate was slightly improved, the heat resistance was enhanced, and the molding shrinkage was slightly reduced, indicating that the silicone foamed microspheres have a significant improvement on the heat resistance and mechanical strength of the composite materials.

[0064] In Example 13, compared with Example 11, carbon nanotubes are used to replace halloysite nanotubes and montmorillonite. The molding shrinkage of the composite material is significantly increased, and the mechanical strength is slightly decreased.

[0065] In Example 14 compared with Example 11, the halloysite nanotubes and montmorillonite were not subjected to amino treatment, and thus could not be chemically connected with the carboxylated silicone foam microspheres, the melt flow rate was reduced, the mechanical strength was affected, and the molding effect was deteriorated.

[0066] In Comparative Example 1, the filler was not modified. Compared with Example 1, the melt flow rate of the composite material increased, but the micropore softening temperature decreased, the heat resistance decreased, and the mechanical properties weakened.

[0067] No mixed fiber was added in Comparative Example 2, and no silicone foamed microspheres were added in Comparative Example 3. Compared with Example 1, the fluidity of the composite material increased, but the heat resistance decreased, the dimensional stability decreased, and the mechanical properties deteriorated.

[0068] Compared with Example 1, Comparative Example 4 uses ABS resin instead of thermoplastic polyurethane. Table 2 shows that the fluidity of the composite material prepared in Comparative Example 4 is significantly reduced and the dimensional stability is decreased.

[0069] Comparative Example 5 is a method for preparing an ABS material provided by the prior art, which has good tensile strength, but its impact resistance and Vicat softening point are not as good as those of the present application, and its heat resistance is insufficient.

[0070] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. A heat-resistant ABS composite material for automobiles, characterized in that: The invention comprises the following raw materials in parts by weight: 80-90 parts of ABS resin, 10-20 parts of thermoplastic polyurethane, 10-20 parts of modified filler, 5-15 parts of organic silicon foam microspheres, 0.1-1 parts of lubricant, 0.1-1 parts of antioxidant, 1-2 parts of flame retardant and 3-8 parts of mixed fiber.

2. The heat-resistant ABS composite material for automobiles according to claim 1, characterized in that: The silicone foamed microspheres are pretreated as follows: The organic silicon foam microspheres are immersed in a concentrated nitric acid solution, reacted at 80-85° C. for 1-2 hours, and vacuum dried to obtain carboxylated organic silicon foam microspheres; In parts by weight, 25-30 parts of halloysite nanotubes and 25-30 parts of montmorillonite are subjected to amination modification to obtain an amination mixture, the amination mixture is added to 200-250 parts of DMF solution, ultrasonicated to obtain a suspension, 400-500 parts of carboxylated silicone foam microspheres and 40-50 parts of phosphate are added, stirred at room temperature for 20-24 hours, filtered, and vacuum dried.

3. The heat-resistant ABS composite material for automobiles according to claim 2, characterized in that: The amination modification of the halloysite nanotubes and montmorillonite is modification with a silane coupling agent.

4. The heat-resistant ABS composite material for automobiles according to claim 1, characterized in that: The mixed fiber comprises basalt fiber and polyetheretherketone fiber in a mass ratio of 0.1-0.3:

1.

5. The heat-resistant ABS composite material for automobiles according to claim 4, characterized in that: The mixed fibers are pretreated as follows: The mixed fiber is treated with a sodium dodecylbenzene sulfonate solution with a concentration of 4-5wt%, and then dispersed in deionized water after drying, and silica sol and agarose are added, and the temperature is raised to 85-90°C, mixed evenly, and then freeze-dried, and then heated to 380-400°C, and kept warm for 2-2.5h to form a fiber skeleton, and the mass ratio of the mixed fiber, silica sol and agarose is 1:6-8:0.25-0.3; The fiber skeleton is added into a 4-5wt% hexadecyltrimethylammonium chloride solution for immersion modification, washed, dried, and crushed to 3-6 mm.

6. The heat-resistant ABS composite material for automobiles according to claim 1, characterized in that: The modified filler comprises hollow glass microspheres with a particle size of 10-45 μm, acrylic artificial stone waste powder with a particle size of 100-125 μm and nano silicon dioxide with a diameter of ≤50 nm in a mass ratio of 0.3-0.6:0.1-0.3:

1.

7. The heat-resistant ABS composite material for automobiles according to claim 6, characterized in that: The modified filler is prepared as follows: polyethersulfone is added to dichloromethane, stirred and dissolved, and a modified liquid with a concentration of 8-10wt% is prepared; Hollow glass microspheres, acrylic artificial stone waste powder and nano-silicon dioxide are mixed to prepare mixed powder, which is added to the modified liquid, stirred for 2-4 hours, dried at 210-230°C for 3-4 hours, and crushed. The amount of mixed powder added is 4-5wt% of the amount of the modified liquid.

8. The heat-resistant ABS composite material for automobiles according to claim 1, characterized in that: The melt index of the ABS is 40-50 g / 10 min.

9. The heat-resistant ABS composite material for automobiles according to claim 1, characterized in that: The antioxidant is one or more of pentaerythritol tetrakis(β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), 4,4'-thiobis(6-tert-butyl-3-methylphenol) and 2-hydroxy-4-n-octyloxybenzophenone; The flame retardant is one or more of triphenyl phosphate, melamine cyanurate, and inorganic filler; The lubricant is one or more of silicone oil, white mineral oil, fatty acid amide, stearate, paraffin, polyethylene wax or ethylene bisstearamide.

10. The method for preparing the heat-resistant ABS composite material for automobiles according to any one of claims 1 to 9, characterized in that: The following steps are involved: Dry the ABS resin and thermoplastic polyurethane at 80-90°C for 6-8h, mix them evenly, extrude and granulate them to make mixed masterbatch; The mixed masterbatch, modified filler, organic silicon foam microsphere, lubricant, antioxidant, flame retardant and mixed fiber are uniformly mixed, extruded and granulated to obtain a composite material.