Polyformaldehyde composite material as well as preparation method and application thereof

By adding ultra-high molecular weight polyethylene and polytetrafluoroethylene to the polyformaldehyde composite material, combined with melt blending and extrusion granulation technology, the problems of low strength and poor toughness of polyformaldehyde materials are solved, and the wear resistance of the material is achieved Improved performance and resilience, suitable for a variety of high-end applications.

CN118931102APending Publication Date: 2024-11-12CHINA ENERGY GRP NINGXIA COAL IND CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411177813.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing polyformaldehyde composite materials have problems such as low strength, poor toughness or poor wear resistance, which cannot meet the needs of high-end products.

Method used

The composite material is prepared by melt blending and extrusion granulation process using a combination of polyformaldehyde, polyethylene, polytetrafluoroethylene, polyethylene glycol, stearate, metal salt, nucleating agent, antioxidant and binder. , improve its wear resistance and toughness.

Benefits of technology

It significantly improves the wear resistance, rigidity and toughness of polyformaldehyde composite materials, and has excellent comprehensive performance. It is suitable for chemical instruments, mechanical equipment and artificial intelligence fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005011210940000071
    Figure BDA0005011210940000071
Patent Text Reader

Abstract

The invention provides a polyformaldehyde composite material as well as a preparation method and application thereof. The polyformaldehyde composite material comprises the following components: polyformaldehyde, polyethylene, polytetrafluoroethylene, polyethylene glycol, stearate, metal salt, a nucleating agent, an antioxidant, a lubricant and an adhesive, wherein the polymerization degree of the polyethylene ranges from 100000 to 200000, and the weight-average molecular weight of the polyethylene ranges from 1000000 to 2000000 Da. The polyformaldehyde material effectively solves the problem of low strength or poor toughness or poor wear resistance of the polyformaldehyde material in the prior art.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of polymer material modification, and in particular to a polyoxymethylene composite material and a preparation method and application thereof. Background Art

[0002] As a thermoplastic, polyoxymethylene resin (POM) has a regular molecular chain configuration, which makes it crystallize quickly and have a high degree of crystallinity (about 60-80%) during melt processing. It is easy to form large spherulites, which gives it excellent mechanical properties. It is one of the types of engineering plastics with mechanical properties closest to metal materials. It can replace metal materials such as steel, copper, zinc, and aluminum in many fields. At the same time, POM also has the advantages of high strength, strong rigidity, wear resistance, creep resistance, fatigue resistance, oil resistance, chemical resistance, self-lubrication, good electrical properties and dimensional stability. It can be used for a long time in the temperature range of -40 to 100°C and is widely used in industrial machinery, automobiles, electronic appliances, agriculture, light industry, chemicals, building materials, water conservancy, agricultural and forestry irrigation, daily consumer goods and other fields. With the widespread application of polyoxymethylene in many fields, such as engineering transmission machinery and equipment, chemical instrument parts, robot joints, new energy vehicles, aerospace and other cutting-edge high-end fields, the toughness and wear resistance of general polyoxymethylene can no longer meet the needs of these high-end products. Therefore, a strong and wear-resistant polyoxymethylene composite material and its preparation method have become an urgent need in the current research field.

[0003] The Chinese invention patent CN107353576A in the prior art discloses a low-odor, high-wear-resistant polyoxymethylene reinforced composite material and its preparation method, and its components mainly include: polyoxymethylene, modified glass fiber, odor adsorption masterbatch, molybdenum disulfide, lubricant, antioxidant. Among them, the invention significantly improves the odor and emission characteristics of the material by adding odor adsorption masterbatch, so that the TVOC of the polyoxymethylene reinforced composite material is lower than 40ugC / g, and the wear index of the polyoxymethylene reinforced composite material prepared by the invention is extremely low, showing excellent wear resistance. In addition, the modified glass fiber significantly improves the dispersibility of glass fiber in the polyoxymethylene matrix, so that the polyoxymethylene reinforced composite material has the advantages of less addition of wear-resistant agent, outstanding wear resistance and significantly improved mechanical properties. However, the toughness of the polyoxymethylene reinforced composite material is insufficient, which limits its further application.

[0004] Chinese invention patent CN101654541A discloses a toughened and wear-resistant magnetic polyoxymethylene composite material, wherein polyoxymethylene, magnetic powder lubricant, stabilizer and coupling agent are mixed in two steps according to a certain ratio, and then melt-mixed and granulated by a single screw extruder to obtain the above polyoxymethylene composite material, but the composite material has the problem of low strength. Chinese invention patent CN201010237793 discloses a high-toughness and high-wear-resistant polyoxymethylene composition and its preparation method, wherein the composition of the polyoxymethylene composition includes: polyoxymethylene 48.0-84.4wt%, polyethylene oxide 10.0-30.0wt%, polytetrafluoroethylene fiber 5.0-20.0wt%, antioxidant 1010 0.25-0.5wt%, antioxidant 168 0.25-0.5wt%, formaldehyde absorbent 0.1-1.0wt%. The specific preparation method is as follows: polyoxymethylene, polytetrafluoroethylene fiber, and polyethylene oxide are dried, the components of the above ratio are placed in a mixer and fully mixed, and then the mixture is melt blended, extruded, cooled, and granulated through a twin-screw extruder granulator. The polyoxymethylene compound prepared by the invention is suitable for the manufacture of mechanical components with high requirements for impact resistance and wear resistance, but it still has the problem of low strength.

[0005] In summary, the polyoxymethylene composite materials in the prior art have problems such as poor wear resistance, poor rigidity or poor toughness, and it is urgent to provide a polyoxymethylene composite material to improve the above problems. Summary of the invention

[0006] The main purpose of the present invention is to provide a polyoxymethylene composite material and a preparation method and application thereof, so as to solve the problems of low strength, poor toughness or poor wear resistance of polyoxymethylene materials in the prior art.

[0007] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, there is provided a polyoxymethylene composite material, which comprises: polyoxymethylene, polyethylene, polytetrafluoroethylene, polyethylene glycol, stearate, metal salt, nucleating agent, antioxidant, lubricant and adhesive; wherein the degree of polymerization of polyethylene is 100000 to 200000, and the weight average molecular weight is 1000000 to 2000000Da.

[0008] Further, in parts by weight, the polyoxymethylene composite material includes 50 to 65 parts of polyoxymethylene, 2 to 5 parts of polyethylene, 3 to 5 parts of polytetrafluoroethylene, 5 to 10 parts of polyethylene glycol, 0.5 to 2 parts of stearate, 1 to 10 parts of metal salt, 0.1 to 0.5 parts of nucleating agent, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of lubricant and 0.1 to 1 parts of adhesive; preferably, the polyoxymethylene composite material includes 58 to 62 parts of polyoxymethylene, 3 to 5 parts of polyethylene, 3 to 4 parts of polytetrafluoroethylene, 6 to 8 parts of polyethylene glycol, 1 to 2 parts of stearate, 4 to 7 parts of metal salt, 0.1 to 0.5 parts of nucleating agent, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of lubricant and 0.3 to 0.8 parts of adhesive.

[0009] Furthermore, the degree of polymerization of polyoxymethylene is 2000-4000, and the weight average molecular weight is 20000-40000Da; preferably, the degree of polymerization of polytetrafluoroethylene is 2000-3000, and the weight average molecular weight is 20000-30000Da; preferably, the degree of polymerization of polyethylene glycol is 2000-6000, and the weight average molecular weight is 4000-6000Da.

[0010] Furthermore, the stearate is selected from one or more of calcium stearate, zinc stearate or barium stearate; preferably, the metal salt is selected from one or more of magnesium silicate, magnesium hydroxide and calcium stearate; preferably, the binder is diphenylmethane diisocyanate.

[0011] Furthermore, the nucleating agent is polyoxymethylene with a degree of polymerization of 500 to 1000; preferably, the antioxidant is selected from antioxidant 245 and / or antioxidant 1010; preferably, the lubricant is calcium stearate.

[0012] According to another aspect of the present application, a method for preparing a polyformaldehyde composite material is also provided, which comprises: step S1, mixing an adhesive with polyformaldehyde once, adding stearate, metal salt, nucleating agent, antioxidant and lubricant for secondary mixing to obtain a polyformaldehyde composite material precursor; step S2, melt-blending and extruding granulation of the polyformaldehyde composite material precursor with polyethylene, polytetrafluoroethylene and polyethylene glycol in sequence to obtain a polyformaldehyde composite material.

[0013] Furthermore, the temperature of the melt blending treatment is 170-205°C, more preferably 190-205°C, and the time is 0.02-0.1h; preferably, the particle size D50 of the particles obtained by the extrusion granulation treatment is 2-3mm; preferably, the extrusion granulation treatment is carried out in a twin-screw extrusion granulator to perform extrusion granulation treatment on the polyoxymethylene composite material.

[0014] Furthermore, after the melting treatment and before the extrusion granulation, a cooling operation is required. Preferably, the polyethylene, polytetrafluoroethylene and polyethylene glycol are also required to be dried before step S2. More preferably, the drying temperature is 60-80°C and the drying time is 6-8h.

[0015] Furthermore, the stirring speed of the first mixing is 5 to 30 rpm, and the processing time is 0.1 to 0.2 h; the stirring speed of the second mixing is 5 to 30 rpm, and the processing time is 0.1 to 0.2 h.

[0016] According to another aspect of the present application, there is also provided an application of the above-mentioned polyformaldehyde composite material, or the polyformaldehyde composite material obtained by the preparation method of the above-mentioned polyformaldehyde composite material in the fields of chemical instruments, mechanical equipment and artificial intelligence.

[0017] The present application effectively solves the problem that polyoxymethylene materials in the prior art exist or have low strength or poor toughness or poor wear resistance. Compared with the polyoxymethylene material components (polyoxymethylene, stearate, nucleating agent, antioxidant, lubricant and adhesive) in the prior art, polyethylene, polytetrafluoroethylene, polyethylene glycol and metal salt are additionally added, and the molecular weight of the polyethylene exceeds 1,000,000, belonging to the polyethylene of ultra-high molecular weight. It is based on the characteristics of polytetrafluoroethylene having acid and alkali resistance, resistance to various organic solvents, high temperature resistance, non-stick, self-lubricating and excellent dielectric properties, especially its friction coefficient is extremely low, has outstanding comprehensive performance, thereby can further improve the wear resistance of polyoxymethylene composite material. In addition, the material has strong rigidity, large hardness and strong toughness, excellent comprehensive performance, and has a wider application field. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] According to the background technology of the present invention, the polyoxymethylene materials in the prior art have the problems of low strength, poor toughness or poor wear resistance. The present invention provides a polyoxymethylene composite material, which comprises: polyoxymethylene, polyethylene, polytetrafluoroethylene, polyethylene glycol, stearate, metal salt, nucleating agent, antioxidant, lubricant and adhesive; wherein the degree of polymerization of the polyethylene is 100000-200000, and the weight average molecular weight is 1000000-2000000Da.

[0020] The polyoxymethylene composite material provided by the present invention, compared to the polyoxymethylene material components (polyoxymethylene, stearate, nucleating agent, antioxidant, lubricant and adhesive) in the prior art, also additionally adds polyethylene, polytetrafluoroethylene, polyethylene glycol and metal salt, and the molecular weight of the polyethylene exceeds 1,000,000, belonging to the polyethylene of ultra-high molecular weight. It is based on the characteristics that polytetrafluoroethylene has acid and alkali resistance, resistance to various organic solvents, high temperature resistance, non-stick, self-lubrication and excellent dielectric properties, especially its friction coefficient is extremely low, has outstanding comprehensive performance, thus can further improve the wear resistance of the polyoxymethylene composite material. Combined with the excellent low temperature resistance of polyethylene, excellent chemical stability and excellent electrical insulation, especially the polyethylene of ultra-high molecular weight is adopted in the present invention, which is 6 times higher than PTFE, 10 times that of carbon steel, and its self-lubricating performance is excellent, and wear is low. Therefore, the polyethylene of ultra-high molecular weight and polytetrafluoroethylene synergistic effect in the polyoxymethylene composite material in the present invention overcomes the defect of poor wear resistance of the polyoxymethylene material in the prior art. At the same time, the polyoxymethylene composite material in the present invention also contains polyethylene glycol, which has good compatibility with water and many organic components, and has excellent lubricity, moisture retention, dispersibility and adhesion, thereby further improving the impact resistance of the polyoxymethylene composite material in the present invention and enhancing its toughness. The metal salt component, due to its strong hardness, high strength, good sintering property, acid and alkali resistance and waterproofness, further enhances the hardness and rigidity in the polyoxymethylene composite material, thereby making the polyoxymethylene composite material have balanced performance, and has excellent wear resistance, strong rigidity, high hardness and strong toughness, excellent comprehensive performance, and has a wider application field.

[0021] In a preferred embodiment, the polyoxymethylene composite material comprises, by weight, 50 to 65 parts of polyoxymethylene, 2 to 5 parts of polyethylene, 3 to 5 parts of polytetrafluoroethylene, 5 to 10 parts of polyethylene glycol, 0.5 to 2 parts of stearate, 1 to 10 parts of metal salt, 0.1 to 0.5 parts of nucleating agent, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of lubricant and 0.1 to 1 parts of adhesive; preferably, the polyoxymethylene composite material comprises 58 to 62 parts of polyoxymethylene, 3 to 5 parts of polyethylene, 3 to 4 parts of polytetrafluoroethylene, 6 to 8 parts of polyethylene glycol, 1 to 2 parts of stearate, 4 to 7 parts of metal salt, 0.1 to 0.5 parts of nucleating agent, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of lubricant and 0.3 to 0.8 parts of adhesive. Under the above dosage ratio, the comprehensive performance of the polyoxymethylene composite material is further improved, the strength is increased, the toughness is enhanced, and the wear resistance is further improved.

[0022] In order to further improve the stability of the polyoxymethylene composite material and make its mechanical properties more stable, the degree of polymerization of polyoxymethylene is preferably 2000-4000, and the weight average molecular weight is 20000-40000Da, and the degree of polymerization of polytetrafluoroethylene is preferably 2000-3000, and the weight average molecular weight is 20000-30000Da, thereby improving the wear resistance of the polyoxymethylene composite material. The degree of polymerization of polyethylene glycol is preferably 2000-6000, and the weight average molecular weight is 4000-6000Da, so as to further improve the toughness of the polyoxymethylene composite material, balance its various properties, and have better comprehensive performance.

[0023] In a preferred embodiment, the stearate is selected from one or more of calcium stearate, zinc stearate or barium stearate, and the metal salt is preferably selected from one or more of magnesium silicate, magnesium hydroxide, and calcium stearate; thereby improving the rigidity of the polyformaldehyde composite material, and improving its strength and impact resistance; in order to further promote the compatibility of each component in the polyformaldehyde composite material with the polyformaldehyde matrix, the preferred adhesive is diphenylmethane diisocyanate.

[0024] In order to further improve the transformation from homogeneous nucleation to heterogeneous nucleation during the formation of the polyoxymethylene composite material, accelerate the crystallization rate, refine the grain structure, and thus improve the rigidity of the polyoxymethylene composite material, the nucleating agent is preferably selected from polyoxymethylene with a degree of polymerization of 500 to 1000; in order to further prevent the polyoxymethylene composite material from being oxidized and decomposed, and improve the comprehensive performance of the polyoxymethylene composite material, the antioxidant is preferably selected from antioxidant 245 and / or antioxidant 1010; at the same time, in order to further improve the compatibility of the polyoxymethylene composite material, increase the density of the product, that is, enhance the rigidity, the lubricant is preferably calcium stearate.

[0025] Another aspect of the present invention provides a method for preparing a polyoxymethylene composite material, the method comprising: step S1, mixing an adhesive with polyoxymethylene, adding stearate, metal salt, nucleating agent, antioxidant and lubricant to obtain a polyoxymethylene composite material precursor; step S2, melt blending the polyoxymethylene composite material precursor with polyethylene, polytetrafluoroethylene and polyethylene glycol in sequence, extruding and granulating to obtain a polyoxymethylene composite material. By adopting the preparation method, the polyoxymethylene composite material has balanced performance, excellent wear resistance, strong rigidity, high hardness and strong toughness, excellent comprehensive performance, and has a wider application field.

[0026] Those skilled in the art may first mix the binder with polyoxymethylene, then add stearate, metal salt, nucleating agent, antioxidant, and lubricant and mix again to obtain a polyoxymethylene composite material precursor; then, melt blend the polyoxymethylene composite material precursor with polyethylene, polytetrafluoroethylene, and polyethylene glycol in sequence, and perform extrusion granulation operations to finally obtain a polyoxymethylene composite material. The preparation method of the polyoxymethylene composite material of the present invention has the characteristics of simple operation and mild conditions, so it is suitable for large-scale preparation and has broad application prospects.

[0027] In a preferred embodiment, the temperature of the melt blending treatment is 170-205°C, more preferably 190-205°C, and the time is 0.02-0.1h; thereby, the compatibility of the above-mentioned raw materials can be improved, thereby improving the rigidity of the polyoxymethylene composite material; in order to better apply the polyoxymethylene composite material to many fields, the particle size D50 obtained by extrusion granulation treatment is preferably 2-3mm; further preferably, the extrusion granulation treatment is carried out in a twin-screw extruder granulator to granulate the polyoxymethylene composite material.

[0028] In order to further prevent the segregation of the material after the melt treatment, thereby further improving the stability of the product after extrusion granulation, it is preferred that a cooling operation is performed after the melt treatment and before the extrusion granulation; at the same time, in order to further improve the rigidity and wear resistance of the polyoxymethylene composite material, it is preferred that the polyethylene, polytetrafluoroethylene and polyethylene glycol are also dried before step S2, and it is further preferred that the drying temperature is 60-80°C and the drying time is 6-8h; it is preferred that the stirring speed of the first mixing is 5-30rpm, the processing time is 0.1-0.2h, and the stirring speed of the second mixing is 5-30rpm, and the processing time is 0.1-0.2h, so that the raw materials of the polyoxymethylene composite material are mixed evenly, the stability of the polyoxymethylene composite material is further improved, and its comprehensive performance is better.

[0029] Another aspect of the present invention provides an application of a polyoxymethylene composite material in chemical instruments, mechanical equipment and artificial intelligence fields. The polyoxymethylene composite material has excellent wear resistance, rigidity and toughness, so that its comprehensive performance is better and its application field is wider.

[0030] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0031] Example 1

[0032] Take adhesive and polyformaldehyde and mix once, stirring speed is 50rpm, time is 0.2h, adhesive is diphenylmethane diisocyanate. Then, stearate, metal salt, nucleator, antioxidant and lubricant are added for secondary mixing, stirring speed is 50rpm, time is 0.2h. Wherein, polyformaldehyde is that degree of polymerization is 2000, weight average molecular weight is 20000Da, stearate is calcium stearate, metal salt is a mixture of magnesium hydroxide and magnesium silicate weight ratio 1: 1, nucleator is polyformaldehyde micropowder with degree of polymerization of about 600, antioxidant is antioxidant 245, lubricant is calcium stearate, and polyformaldehyde composite material precursor is obtained.

[0033] Then, polyethylene, polytetrafluoroethylene and polyethylene glycol were dried at a temperature of 100°C for 4 hours. The polyoxymethylene composite precursor was melt blended with polyethylene, polytetrafluoroethylene and polyethylene glycol at 195°C for 0.2 hours, and then extruded and granulated in a twin-screw extruder granulator after cooling to obtain a polyoxymethylene composite material with a particle size D50 of 2 to 3 mm. Among them, the degree of polymerization of polyethylene is 100,000 and the molecular weight is 1,000,000 Da, the degree of polymerization of polytetrafluoroethylene is 2,000 and the molecular weight is 20,000 Da, and the degree of polymerization of polyethylene glycol is 2,000 and the molecular weight is 20,000 Da.

[0034] The components of the polyoxymethylene composite material are as follows by weight: 65 parts of polyoxymethylene, 5 parts of polyethylene, 5 parts of polytetrafluoroethylene, 10 parts of polyethylene glycol, 2 parts of stearate, 10 parts of metal salt, 0.5 parts of nucleating agent, 0.5 parts of antioxidant, 0.5 parts of lubricant and 1 part of adhesive.

[0035] Example 2

[0036] The difference from Example 1 is that the proportions of the components are different:

[0037] The components of the polyoxymethylene composite material are as follows by weight: 50 parts of polyoxymethylene, 2 parts of polyethylene, 3 parts of polytetrafluoroethylene, 5 parts of polyethylene glycol, 0.5 parts of stearate, 1 part of metal salt, 0.1 parts of nucleating agent, 0.1 parts of antioxidant, 0.1 parts of lubricant and 0.1 parts of adhesive.

[0038] Example 3

[0039] The difference from Example 1 is that the proportions of the components are different:

[0040] The components of the polyoxymethylene composite material are as follows by weight: 65 parts of polyoxymethylene, 5 parts of polyethylene, 4 parts of polytetrafluoroethylene, 8 parts of polyethylene glycol, 2 parts of stearate, 7 parts of metal salt, 0.5 parts of nucleating agent, 0.5 parts of antioxidant, 0.5 parts of lubricant and 0.8 parts of adhesive.

[0041] Example 4

[0042] The difference from Example 1 is that the proportions of the components are different:

[0043] The components of the polyoxymethylene composite material are as follows by weight: 58 parts of polyoxymethylene, 3 parts of polyethylene, 3 parts of polytetrafluoroethylene, 6 parts of polyethylene glycol, 1 part of stearate, 4 parts of metal salt, 0.1 part of nucleating agent, 0.1 part of antioxidant, 0.1 part of lubricant and 0.3 part of adhesive.

[0044] Comparative Example 1

[0045] The only difference from Example 1 is that no polyethylene is added.

[0046] Comparative Example 2

[0047] The only difference from Example 1 is that no polytetrafluoroethylene is added.

[0048] Comparative Example 3

[0049] The only difference from Example 1 is that polyethylene and polytetrafluoroethylene are not added.

[0050] Comparative Example 4

[0051] The only difference from Example 1 is that no polyethylene glycol is added.

[0052] Comparative Example 5

[0053] The only difference from Example 1 is that no stearate and metal salt are added.

[0054] Comparative Example 6

[0055] The only difference from Example 1 is that no nucleating agent, antioxidant, lubricant, acid absorbent and adhesive are added.

[0056] Comparative Example 7

[0057] 100 wt % polyoxymethylene was directly injection molded into standard specimen bars for analysis and testing.

[0058] Performance Test:

[0059] 1. Friction coefficient

[0060] According to GB / T3960 standard test, M-200 wear tester was used to test the friction coefficient for 2 hours at a load of 20kg and a speed of 200r / min.

[0061] 2. Mechanical properties

[0062] (1) The specimens were conditioned under constant temperature (temperature, 23±2°C) and constant humidity (relative humidity, RH 50%±5%) conditions; (2) The tensile performance test was conducted on a universal material testing machine in accordance with GB / T 1040.2-2006 standard, with a tensile rate of 50mm / min; (3) The bending performance test was conducted on a universal material testing machine in accordance with GB / T 9341-2008 standard, with a bending test rate of 2mm / min and a bending test span of 64mm. (4) The test specimens were notched according to GB / T1043.1-2008 and tested on an impact testing machine. The simply supported beam notch impact test used a 0.5J pendulum,

[0063] The polyoxymethylene composite materials prepared in the above comparative examples and embodiments were processed into standard test specimens for tensile, bending, impact and wear resistance under unified injection molding conditions, and the performance test results were as follows.

[0064] Table 1

[0065]

[0066] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A polyoxymethylene composite material, characterized in that: The polyoxymethylene composite material comprises: polyoxymethylene, polyethylene, polytetrafluoroethylene, polyethylene glycol, stearate, metal salt, nucleating agent, antioxidant, lubricant and adhesive; wherein the polymerization degree of the polyethylene is 100000-200000, and the weight average molecular weight is 1000000-2000000Da.

2. The polyoxymethylene composite material according to claim 1, characterized in that: The polyoxymethylene composite material comprises, by weight, 50 to 65 parts of the polyoxymethylene, 2 to 5 parts of the polyethylene, 3 to 5 parts of the polytetrafluoroethylene, 5 to 10 parts of the polyethylene glycol, 0.5 to 2 parts of the stearate, 1 to 10 parts of the metal salt, 0.1 to 0.5 parts of the nucleating agent, 0.1 to 0.5 parts of the antioxidant, 0.1 to 0.5 parts of the lubricant and 0.1 to 1 parts of the adhesive; Preferably, the polyoxymethylene composite material includes 58 to 62 parts of the polyoxymethylene, 3 to 5 parts of the polyethylene, 3 to 4 parts of the polytetrafluoroethylene, 6 to 8 parts of the polyethylene glycol, 1 to 2 parts of the stearate, 4 to 7 parts of the metal salt, 0.1 to 0.5 parts of the nucleating agent, 0.1 to 0.5 parts of the antioxidant, 0.1 to 0.5 parts of the lubricant and 0.3 to 0.8 parts of the adhesive.

3. The polyoxymethylene composite material according to claim 1 or 2, characterized in that: The degree of polymerization of the polyoxymethylene is 2000-4000, and the weight average molecular weight is 20000-40000Da; Preferably, the degree of polymerization of the polytetrafluoroethylene is 2000-3000, and the weight average molecular weight is 20000-30000Da; Preferably, the degree of polymerization of the polyethylene glycol is 2000-6000, and the weight average molecular weight is 4000-6000 Da.

4. The polyoxymethylene composite material according to any one of claims 1 to 3, characterized in that: The stearate is selected from one or more of calcium stearate, zinc stearate or barium stearate; Preferably, the metal salt is selected from one or more of magnesium silicate, magnesium hydroxide and calcium stearate; Preferably, the binder is diphenylmethane diisocyanate.

5. The polyoxymethylene composite material according to any one of claims 1 to 4, characterized in that: The nucleating agent is polyoxymethylene with a degree of polymerization of 500 to 1000; Preferably, the antioxidant is selected from antioxidant 245 and / or antioxidant 1010; Preferably, the lubricant is calcium stearate.

6. A method for preparing a polyoxymethylene composite material according to any one of claims 1 to 5, characterized in that: The preparation method comprises: Step S1, mixing the adhesive and polyoxymethylene once, adding stearate, metal salt, nucleating agent, antioxidant and lubricant for secondary mixing to obtain a polyoxymethylene composite material precursor; Step S2, melt-blending the polyoxymethylene composite material precursor with polyethylene, polytetrafluoroethylene and polyethylene glycol in sequence, and extruding and granulating to obtain the polyoxymethylene composite material.

7. The method for preparing the polyoxymethylene composite material according to claim 6, characterized in that: The temperature of the melt blending treatment is 170-205°C, more preferably 190-205°C, and the time is 0.02-0.1h; Preferably, the particle size D50 of the particles obtained by the extrusion granulation process is 2 to 3 mm; Preferably, the extrusion granulation process is carried out in a twin-screw extrusion granulator to perform an extrusion granulation process on the polyoxymethylene composite material.

8. The method for preparing the polyoxymethylene composite material according to claim 6 or 7, characterized in that: After the melting process and before the extrusion granulation, a cooling operation is required. Preferably, the polyethylene, the polytetrafluoroethylene and the polyethylene glycol need to be dried before step S2. More preferably, the drying temperature is 60 to 80°C and the drying time is 6 to 8 hours.

9. The method for preparing the polyoxymethylene composite material according to claim 8, characterized in that: The stirring speed of the primary mixing is 5 to 30 rpm, and the processing time is 0.1 to 0.2 h; The stirring speed of the secondary mixing is 5 to 30 rpm, and the processing time is 0.1 to 0.2 h.

10. Use of the polyoxymethylene composite material according to any one of claims 1 to 5, or the polyoxymethylene composite material obtained by the preparation method of the polyoxymethylene composite material according to any one of claims 6 to 9 in the fields of chemical instruments, mechanical equipment and artificial intelligence.