Three-phase composite material and preparation method and application thereof

By filling the hollow glass microbead composite foam with the most closely packed and arranged carbon fiber tubes, the problem of insufficient compressive performance of traditional solid buoyant materials is solved, and a three-phase composite material with smaller density and higher compressive performance is achieved. Extended its application scope.

CN118931109APending Publication Date: 2024-11-12HARBIN ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411147256.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional solid buoyant materials are difficult to effectively improve the compressive performance of the material by doping discontinuous fibers, which limits their application range.

Method used

Fill in hollow glass microbead composite foam with the most closely packed and arranged carbon fiber tubes, and prepare three-phase composite materials in combination with low-temperature and high-temperature curing techniques to improve the overall specific strength and compressive resistance of the material.

Benefits of technology

The three-phase composite material with a smaller density has good compressive resistance, is suitable for applications with a depth of 500m, and expands the application range of solid buoyancy materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931109A_ABST
    Figure CN118931109A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of solid buoyancy materials, and particularly relates to a three-phase composite material and a preparation method and application thereof. The three-phase composite material provided by the invention comprises hollow glass bead composite foam and a plurality of carbon fiber tubes filled in the hollow glass bead composite foam, the carbon fiber tubes are arranged in a two-dimensional close packing manner, the center-to-center distance between every two adjacent carbon fiber tubes is 29.9-34 mm, and the wall thickness of each carbon fiber tube is 0.45-1 mm; and two ends of the carbon fiber tube are sealed by end caps. The three-phase composite material provided by the invention has relatively small density (0.2-0.4 g / cm < 3 >) and good compression resistance, and has 500m water depth use performance under 3 times of safety coefficient.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of solid buoyancy materials, and in particular relates to a three-phase composite material and a preparation method and application thereof. Background Art

[0002] Solid buoyancy material is a lightweight material with low density and high strength. Most traditional solid buoyancy materials are two-phase epoxy synthetic foams made by infusing glass microspheres with epoxy resin. In order to further reduce the density of solid buoyancy materials, three-phase composite buoyancy materials have been proposed, usually by doping discontinuous fibers to achieve the purpose of reducing material density or improving material strength. However, the improvement of material specific strength by doping discontinuous fibers is limited, thus limiting its scope of application. Summary of the invention

[0003] In view of this, the present invention provides a three-phase composite material and a preparation method and application thereof. The three-phase composite material provided by the present invention has better compressive resistance while having a smaller density, thereby expanding its application range as a solid buoyancy material.

[0004] In order to solve the above technical problems, the present invention provides a three-phase composite material, including a hollow glass microsphere composite foam and a plurality of carbon fiber tubes filled in the hollow glass microsphere composite foam;

[0005] The carbon fiber tubes are arranged in a two-dimensional closest packing, the center distance between two adjacent carbon fiber tubes is 29.9-34 mm, the wall thickness of the carbon fiber tubes is 0.45-1 mm; and both ends of the carbon fiber tubes are sealed by end caps.

[0006] Preferably, the cross-sectional shape of the standard piece of the three-phase composite material is circular, hexagonal or square, and the height of the standard piece of the three-phase composite material is 150-500 mm.

[0007] Preferably, the inner diameter of the carbon fiber tube is 26-30 mm.

[0008] Preferably, the method for preparing the carbon fiber tube comprises the following steps:

[0009] The thin carbon fiber prepreg and the thick carbon fiber prepreg are orthogonally laid in the direction of the carbon fibers and then rolled to obtain a tube blank; the thickness ratio of the thin carbon fiber prepreg and the thick carbon fiber prepreg is 1:2;

[0010] The carbon fiber tube is obtained by winding a biaxially oriented polypropylene film on the surface of the tube blank, curing the film, and demoulding the film to obtain the carbon fiber tube.

[0011] Preferably, the curing includes low-temperature curing and high-temperature curing performed sequentially, the temperature of the low-temperature curing is 75-85°C, and the time of the low-temperature curing is 25-35 minutes; the temperature of the high-temperature curing is 120-140°C, and the time of the high-temperature curing is 110-130 minutes.

[0012] Preferably, the end cap is made of carbon fiber, titanium alloy or aluminum alloy, and is in the shape of a sheet or a hemispherical shell.

[0013] Preferably, the density of the hollow glass microsphere composite foam is 0.4-0.5 g / cm 3 .

[0014] The present invention also provides a method for preparing the three-phase composite material described in the above technical solution, including method 1 and method 2;

[0015] The method 1 comprises the following steps:

[0016] preparing a mold according to the shape of the three-phase composite material;

[0017] Arranging the carbon fiber tubes in a mold, pouring a mixture of glass beads and epoxy resin, and curing and molding to obtain the three-phase composite material;

[0018] The method 2 comprises the following steps:

[0019] Processing the solidified hollow glass microsphere composite foam to obtain a hollow glass microsphere composite foam containing pores;

[0020] The carbon fiber tube is embedded in the hole and sealed and bonded to obtain the three-phase composite material.

[0021] Preferably, the sealing adhesive comprises epoxy resin.

[0022] The present invention also provides the use of the three-phase composite material described in the above technical solution or the three-phase composite material prepared by the preparation method described in the above technical solution as a buoyancy material.

[0023] The present invention provides a three-phase composite material, including a hollow glass microsphere composite foam and a plurality of carbon fiber tubes filled in the hollow glass microsphere composite foam; the carbon fiber tubes are arranged in a two-dimensional closest packing, the center spacing between two adjacent carbon fiber tubes is 29.9 to 34 mm, and the wall thickness of the carbon fiber tube is 0.45 to 1 mm; the two ends of the carbon fiber tube are sealed by end caps. The present invention further improves the overall specific strength of the material by placing a two-dimensional closest packed high-strength carbon fiber tube in the traditional two-phase solid buoyancy material hollow glass microsphere composite foam. In the present invention, the continuous fibers in the carbon fiber tube (prepared from carbon fiber prepreg) improve the bearing capacity of the three-phase composite material. At the same time, the present invention limits the center spacing between adjacent carbon fiber tubes within a certain range to improve the hydrostatic strength of the material, thereby improving the compressive performance of the three-phase composite material structure. The three-phase composite material provided by the present invention has a relatively small density (0.2 to 0.4 g / cm 3 ), and has good pressure resistance, and can be used in 500m water depth with a safety factor of 3. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the process of preparing carbon fiber tubes and three-phase composite materials using method 2 as an example;

[0025] Figure 2 Schematic diagram of the structure of the three-phase composite material prepared in Example 1, wherein 1 is a carbon fiber tube and 2 is a hollow glass microsphere composite foam;

[0026] Figure 3 1 is an exploded view of the structural schematic diagram of the three-phase composite material prepared in Example 1, wherein 1 is a carbon fiber tube, 2 is a hollow glass microsphere composite foam, and 3 is an end cap;

[0027] Figure 4 This is a physical picture of the three-phase composite material prepared in Example 1. DETAILED DESCRIPTION

[0028] The invention provides a three-phase composite material, comprising hollow glass microsphere composite foam and a plurality of carbon fiber tubes filled in the hollow glass microsphere composite foam.

[0029] In the present invention, the carbon fiber tubes are arranged in a two-dimensional closest packing in the hollow glass microsphere composite foam, and the center distance between two adjacent carbon fiber tubes is 29.9 to 34 mm, preferably 30.4 to 33.5 mm; the wall thickness of the carbon fiber tube is 0.45 to 1 mm, preferably 0.5 to 0.8 mm. In the present invention, the cross-sectional shape of the standard parts of the three-phase composite material is preferably circular, hexagonal or square, more preferably hexagonal. In the present invention, the height of the standard parts of the three-phase composite material is preferably 150 to 500 mm, more preferably 200 to 400 mm. In the present invention, the axes of the carbon fiber tubes in the three-phase composite material are parallel to each other. In the present invention, the inner diameter of the carbon fiber tube is preferably 24 to 30 mm, more preferably 27 mm.

[0030] In the present invention, both ends of the carbon fiber tube are sealed by end caps; the material of the end caps is preferably carbon fiber, titanium alloy or aluminum alloy, more preferably carbon fiber; the shape of the end caps is preferably sheet-like or hemispherical shell-like, more preferably sheet-like. In the present invention, the shape of the end caps is preferably consistent with the cross-sectional shape of the carbon fiber tube, and the thickness of the end caps is preferably 2.4 to 4 mm, more preferably 2.8 to 3.4 mm.

[0031] In the present invention, the method for preparing the carbon fiber tube preferably comprises the following steps:

[0032] The thin carbon fiber prepreg and the thick carbon fiber prepreg are orthogonally laid in the direction of the carbon fibers and then rolled to obtain a tube blank; the thickness ratio of the thin carbon fiber prepreg and the thick carbon fiber prepreg is 1:2;

[0033] The carbon fiber tube is obtained by winding a biaxially oriented polypropylene film on the surface of the tube blank, curing the film, and demoulding the film to obtain the carbon fiber tube.

[0034] The present invention rolls up a thin layer of carbon fiber prepreg and a thick layer of carbon fiber prepreg after orthogonal plying in the direction of the carbon fibers to obtain a tube blank. In the present invention, the carbon fiber prepreg used to prepare the carbon fiber tube is preferably purchased from Shandong Kehang New Materials Co., Ltd., and the resin content in the carbon fiber prepreg is preferably 33-37%, more preferably 35%; the model of the carbon fiber prepreg is preferably T700-12K, and the matrix resin model of the carbon fiber prepreg is preferably KH1301. In the present invention, the thickness ratio of the thin layer of carbon fiber prepreg and the thick layer of carbon fiber prepreg is preferably 1:2. In the present invention, the thickness of the thick layer of carbon fiber prepreg is preferably 0.1mm.

[0035] In the present invention, the carbon fiber prepreg after layering is preferably rolled onto a steel mold. The present invention has no special limitation on the rolling, and a conventional method in the art can be used.

[0036] The present invention rolls thin carbon fiber prepreg and thick carbon fiber prepreg after orthogonally plying them in the direction of carbon fibers, which can ensure the hydrostatic strength of a single carbon tube. In addition, the plying method can achieve better molding quality during the rolling process and is less likely to cause fiber wrinkles.

[0037] After obtaining the tube blank, the present invention winds a biaxially oriented polypropylene film on the surface of the tube blank, solidifies it, and demolds it to obtain the carbon fiber tube. In the present invention, the winding pitch is preferably 2 mm, and the winding tension is preferably 10 N. In the present invention, the biaxially oriented polypropylene film (BOPP) is preferably a heat shrink film, which can provide pressure for the tube blank during curing, which is beneficial to reduce the porosity of the carbon fiber tube and thus ensure the strength of the carbon tube.

[0038] In the present invention, the curing preferably includes low-temperature curing and high-temperature curing performed in sequence, the temperature of the low-temperature curing is preferably 75-85°C, more preferably 80°C; the time of the low-temperature curing is preferably 25-35min, more preferably 30min; the temperature of the high-temperature curing is preferably 120-140°C, more preferably 130°C; the time of the high-temperature curing is preferably 110-130min, more preferably 120min.

[0039] The present invention has no special requirements for the demoulding, and the conventional method in the art can be used.

[0040] In the present invention, the carbon fiber tube includes a circumferential fiber amount and an axial fiber amount stacked in sequence, and the thickness of the circumferential fiber amount is twice the thickness of the axial fiber amount. The carbon fibers in the thin carbon fiber prepreg in the carbon fiber tube are arranged in the axial direction, and the carbon fibers in the thick carbon fiber prepreg in the carbon fiber tube are arranged in the circumferential direction; the orthogonal fiber directions in the carbon fiber tube improve the compressive performance of the carbon fiber tube.

[0041] In the present invention, the hollow glass microsphere composite foam is preferably composed of glass microspheres and epoxy resin, and the density of the hollow glass microsphere composite foam is preferably 0.4-0.5 g / cm 3 , more preferably 0.43 to 0.46 g / cm 3 The tensile strength of the hollow glass microsphere composite foam is preferably 15-20 MPa, the shear strength is preferably 12-18 MPa, and the compressive strength is preferably 24-35 MPa. In the present invention, the hollow glass microsphere composite foam is preferably purchased from Qingdao Haoyi Industrial Co., Ltd.

[0042] The present invention also provides a method for preparing the three-phase composite material described in the above technical solution, including method 1 and method 2.

[0043] In the present invention, the method 1 comprises the following steps:

[0044] preparing a mold according to the shape of the three-phase composite material;

[0045] The carbon fiber tubes are arranged in a mold, and then a mixture of glass microbeads and epoxy resin is poured into the mold, and the three-phase composite material is obtained after curing and molding.

[0046] In the present invention, when pouring the filler, the length of the poured filler preferably exceeds the length of the carbon fiber tube, and the length exceeding the carbon fiber tube is preferably less than or equal to 5 mm, more preferably 1 to 3 mm.

[0047] In the present invention, the method 2 comprises the following steps:

[0048] Processing the solidified hollow glass microsphere composite foam to obtain a hollow glass microsphere composite foam containing pores;

[0049] The carbon fiber tubes are embedded into the holes and sealed and bonded to obtain the three-phase composite material.

[0050] In the present invention, the sealing adhesive preferably includes epoxy resin.

[0051] In the present invention, the processing method is preferably milling.

[0052] Taking method 2 as an example, the schematic diagram of the process for preparing carbon fiber tubes and three-phase composite materials is as follows: Figure 1 As shown, specifically, a thin layer of carbon fiber prepreg and a thick layer of carbon fiber prepreg are orthogonally laid in the direction of carbon fiber and then rolled, a BOPP film is wrapped around the surface of the tube blank by a horizontal wrapping machine, and then cured and demoulded in sequence, the demoulded product is cut and the carbon fiber sheet material is used as an end cap to seal the two ends of the carbon fiber tube; the cured hollow glass microsphere composite foam is cut and then installed and bonded to the carbon fiber tube to obtain a three-phase composite material.

[0053] The present invention also provides the use of the three-phase composite material described in the above technical solution or the three-phase composite material prepared by the preparation method described in the above technical solution as a solid buoyancy material.

[0054] In order to further illustrate the present invention, the technical solutions provided by the present invention are described in detail below in conjunction with embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0055] Example 1

[0056] A thin layer of carbon fiber prepreg (thickness of 0.05 mm, resin content of 35%) and a thick layer of carbon fiber prepreg (thickness of 0.1 mm, resin content of 35%) purchased from Shandong Kehang New Materials Co., Ltd. were rolled up after orthogonal plying in the direction of carbon fibers to obtain a tube blank; the model of the carbon fiber prepreg is T700-12K, and the model of the matrix resin of the carbon fiber prepreg is KH1301;

[0057] After the surface of the tube blank is coated with a biaxially oriented polypropylene film (the winding pitch is 2 mm, and the winding tension is 10 N), the tube blank is low-temperature cured at 80° C. for 30 min, and then high-temperature cured at 130° C. for 120 min, demoulded, cut, and the two ends of the cut material are sealed with a carbon fiber sheet with a thickness of 3.2 mm as an end cap to obtain a carbon fiber tube with an inner diameter of 27 mm, a wall thickness of 0.75 mm, and a length of 150 mm;

[0058] The carbon fiber tubes are arranged in a two-dimensional closest packing arrangement in a mold. The center spacing between adjacent carbon fiber tubes is 31.5 mm. The density of the infusion into the pores of the arrayed carbon fiber tubes is 0.45 g / cm 3 A mixture of glass microspheres and epoxy resin with a tensile strength of 17MP, a shear strength of 15MPa, and a compressive strength of 27MPa (purchased from Qingdao Haoyi Industrial Co., Ltd.) was cured and molded to obtain a three-phase composite material.

[0059] Figure 2 Schematic diagram of the structure of the three-phase composite material prepared in Example 1, wherein 1 is a carbon fiber tube and 2 is a hollow glass microsphere composite foam. Figure 3 Schematic diagram of the explosion of the structure of the three-phase composite material prepared in Example 1, wherein 1 is a carbon fiber tube, 2 is a hollow glass microsphere composite foam, and 3 is an end cap.

[0060] Figure 4 This is a physical picture of the three-phase composite material prepared in Example 1.

[0061] According to the method of GB / T 6342 (Determination of Linear Dimensions of Foam Plastics and Rubber), the dimensions of the three-phase composite material prepared in Example 1 were detected and the equivalent density was calculated by weighing, and the results are listed in Table 1. According to the method of GJB 9435-2018 (Specification for Microbead Resin Composite Solid Buoyancy Materials for Deep Sea), the hydrostatic strength of the three-phase composite material prepared in Example 1 was detected, and the results are listed in Table 1. The three-phase composite material prepared in Example 1 was immersed in water for 24 hours and then its water absorption was detected, and the results are listed in Table 1.

[0062] Table 1 Performance parameters of carbon fiber three-phase composite materials prepared in Example 1

[0063] Example <![CDATA[Equivalent density (g / cm 3 )]]> Hydrostatic strength(MPa) Water absorption (%) Example 1 0.3011 20.33 0.3

[0064] It can be seen from the test results in Table 1 that the three-phase composite material provided by the present invention has a lower equivalent density and good compressive performance.

[0065] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A three-phase composite material, characterized in that: It comprises a hollow glass microsphere composite foam and a plurality of carbon fiber tubes filled in the hollow glass microsphere composite foam; The carbon fiber tubes are arranged in a two-dimensional closest packing, the center distance between two adjacent carbon fiber tubes is 29.9-34 mm, the wall thickness of the carbon fiber tubes is 0.45-1 mm; and both ends of the carbon fiber tubes are sealed by end caps.

2. The three-phase composite material according to claim 1, characterized in that: The cross-sectional shape of the standard piece of the three-phase composite material is circular, hexagonal or square, and the height of the standard piece of the three-phase composite material is 150-500 mm.

3. The three-phase composite material according to claim 1, characterized in that: The inner diameter of the carbon fiber tube is 26-30 mm.

4. The three-phase composite material according to any one of claims 1 to 3, characterized in that: The method for preparing the carbon fiber tube comprises the following steps: The thin carbon fiber prepreg and the thick carbon fiber prepreg are orthogonally laid in the direction of the carbon fibers and then rolled to obtain a tube blank; the thickness ratio of the thin carbon fiber prepreg and the thick carbon fiber prepreg is 1:2; The carbon fiber tube is obtained by winding a biaxially oriented polypropylene film on the surface of the tube blank, curing the film, and demoulding the film to obtain the carbon fiber tube.

5. The three-phase composite material according to claim 4, characterized in that: The curing includes low temperature curing and high temperature curing performed sequentially, wherein the temperature of the low temperature curing is 75-85°C and the time of the low temperature curing is 25-35 minutes; the temperature of the high temperature curing is 120-140°C and the time of the high temperature curing is 110-130 minutes.

6. The three-phase composite material according to claim 1, characterized in that: The material of the end cap is carbon fiber, titanium alloy or aluminum alloy, and the shape of the end cap is sheet-shaped or hemispherical shell-shaped.

7. The three-phase composite material according to claim 1, characterized in that: The density of the hollow glass microsphere composite foam is 0.4-0.5 g / cm 3 .

8. The method for preparing the three-phase composite material according to any one of claims 1 to 7, comprising method 1 and method 2; The method 1 comprises the following steps: preparing a mold according to the shape of the three-phase composite material; Arranging the carbon fiber tubes in a mold, pouring a mixture of glass beads and epoxy resin, and curing and molding to obtain the three-phase composite material; The method 2 comprises the following steps: Processing the solidified hollow glass microsphere composite foam to obtain a hollow glass microsphere composite foam containing pores; The carbon fiber tube is embedded in the hole and sealed and bonded to obtain the three-phase composite material.

9. The preparation method according to claim 8, characterized in that: The sealing adhesive includes epoxy resin.

10. Use of the three-phase composite material according to any one of claims 1 to 7 or the three-phase composite material prepared by the preparation method according to any one of claims 8 to 9 as a buoyancy material.